Alloy 6005A is a medium-strength structural aluminum grade of the 6000 series, designated EN AW-6005A or AlSiMg(A), with a better finish than 6082. Hydro describes it as combining strength, toughness and surface finish. It sits between 6063 and 6082 on most of the maker’s grading lines. Its guaranteed strength falls as the wall gets thicker.Composition
Hydro lists 0.50 to 0.90 % silicon and 0.40 to 0.70 % magnesium for EN AW-6005A. Iron may reach 0.35 % and chromium 0.30 %. A footnote holds manganese and chromium together between 0.12 and 0.50 %. The silicon window sits between those of 6063 and 6082.Read More
Strength Pattern
An open T6 profile with walls up to 5 mm (0.20 in) gets 225 MPa (32.6 ksi) yield. Its tensile floor is 270 MPa (39.2 ksi). Between 5 and 10 mm the yield floor is 215 MPa (31.2 ksi). From 10 to 25 mm (0.39 to 0.98 in) it is 200 MPa (29.0 ksi). Hollow sections start lower, at 215 MPa up to 5 mm. A thicker rib on a 6005A section therefore lowers the figure for the whole profile.North American Rows
Hydro’s sheet lists T4 and T6 only, so it offers no T5 line. The Aluminum Association’s table gives 6005A a T5 at 214 MPa (31.0 ksi) yield and 262 MPa (38.0 ksi) tensile. Its T61 rows reach 241 MPa (35.0 ksi) yield. The temper asked for has to exist in the table that will certify it.Workshop Grades
On Hydro’s relative scale, with 5 at the top, 6005A grades 3 for tensile strength and 4 for machinability. Weldability is 5, decorative anodizing 3 and surface finish 3. For a decorative anodized face, Hydro rates it above 6082. Its listed uses include boat masts, railway sections, train carriages and complex sections for bus and truck structures.Physical Data
The modulus is 70 GPa (10.2 Msi) and the density 2.71 g/cm³ (0.098 lb/in³). The melting range is 605 to 655 °C (1,121 to 1,211 °F). Thermal conductivity in T6 is 176 W/m·K (102 BTU/h·ft·°F). At the press, an Alliance sheet asks for a minimum exit of 510 °C (950 °F) for 6005A, above the figure for 6063.