Drawing6063Aluminum Association

ASTM B221 for Extruded Aluminum Profiles Read for the Buyer

The specification certifies alloy, temper and tensile behavior, so the drawing still has to carry geometry, units and thickness.

A bundle of extruded aluminum profiles tied together, mixed shapes, angles, tubes and channels, satin silver.

In the Aluminum Association’s table of limits for extruded profiles, 6061-T6 keeps the same 241 MPa (35.0 ksi) minimum yield strength whether the wall is 2 mm or 20 mm thick. Only the elongation changes, from 8 % up to a 6.3 mm wall to 10 % above it. 6063-T5 does the opposite and gives up 1.0 ksi of tensile strength and 1.0 ksi of yield when the wall passes 12.7 mm.

Two alloys and two patterns, in a single table. ASTM B221 is the specification whose name a buyer meets on drawings, quotes and mill test reports, often without opening it. The sections below read what the public description of the standard says it covers, what the companion tables give, and what a supplier signs.

What ASTM B221 Covers

ASTM’s catalog page for B221-21, last updated October 29, 2021, describes the standard as a specification for aluminum and aluminum-alloy extruded bars, rods, wire, profiles and tubes. It covers the alloys and tempers listed in its Table 2 and requires the products to be made by hot extrusion or a similar process.

The text on the page names the requirements: chemical composition by specified chemical and spectrochemical methods, sampling from ingots or finished products, and tensile strength, yield strength and elongation. It adds that elongation requirements do not apply below specified size limits.

The metadata of the page gives the shape of the document. It belongs to Committee B07, Subcommittee B07.03, in volume 02.02 of the Book of Standards, runs to 17 pages, and has a DOI of 10.1520/B0221-21. The paragraphs here paraphrase the public catalog description only and do not reproduce the standard’s text or tables.

B221 is a material specification. It certifies composition and tensile behavior of the extruded product, and it leaves the geometry of the profile to the tolerance documents.

What the Standard Points To

The catalog page lists the documents that B221 refers to. Reading that list shows where B221 stops.

Table 1. Neighboring ASTM specifications named in the notes to the scope of B221-21, and what each is named for
Specification Product named in the note
B211 / B211M rolled or cold-finished bar and rod
B210 / B210M drawn tube for pressure use
B429 / B429M structural pipe and tube
B241 / B241M pipe and tube for pressure use
B234 surface condensers, evaporators and heat exchangers
ANSI H35.1 / H35.1M alloy and temper designations
ASTM Practice E527 UNS equivalents of the alloy numbers

Note 3 of the scope says pipe and tube under B221 are for general purposes. The standard may not cover manufacturing, integrity testing or verification for pressurized fluid service, and the note sends that application to B210 or B241.

For a buyer of profile, the table says two things. A hollow extruded section is inside B221 when it is a profile, and it is outside it the moment it has to carry pressure. Tube for a heat exchanger belongs to B234.

Designations, Units and the Companion Standard

Section 1.2 of the scope, as the catalog page shows it, says alloy and temper designations follow ANSI H35.1 and H35.1M, and that the UNS number of an alloy is the Table 1 number prefixed with A9. 6063 becomes A96063 in this scheme. Note 1 says the word alloy is used broadly to include pure aluminum.

Units split the family in two. Section 1.4 says a metric companion, B221M, exists, and that B221 itself gives no metric equivalents. A drawing in millimeters and MPa cites B221M, and a drawing in inches and ksi cites B221, and a mixed drawing needs to say which one governs.

Section 1.3 points to Annex A2 for the criteria by which new aluminum alloys are added, and section 1.5 states that the standard was developed under the WTO principles for international standards. For a purchase order the section that matters is 1.2, since it is where the alloy and temper on the certificate are defined.

Alloy and Temper Limits in the Companion Tables

B221 reaches the buyer through its limits on tensile strength, yield strength and elongation by alloy, temper and thickness. The Aluminum Association’s table of mechanical property limits for extruded wire, rod, bar and profiles, in the May 2009 reprint of Aluminum Standards and Data, is the table the Association itself publishes for the same product form.

The reprint was opened for this piece, and the B221 Table 2 itself was not. Values below are therefore the Association’s, labeled as such, and a buyer who cites B221 checks each row in the current B221 text before relying on it.

Table 2. Mechanical property limits for extruded profiles of four common alloys, Aluminum Association Table 11.1, 2009 reprint. Thickness in millimeters first, inches as printed in brackets; limits in MPa first, ksi as printed in brackets (converted here)
Alloy and temper Specified thickness Tensile, min Yield, min Elongation, min
6061-T4 all 179 MPa (26.0 ksi) 110 MPa (16.0 ksi) 16 %
6061-T6 6.3 mm (up to 0.249 in) 262 MPa (38.0 ksi) 241 MPa (35.0 ksi) 8 %
6061-T6 6.4 mm (0.250 in) and over 262 MPa (38.0 ksi) 241 MPa (35.0 ksi) 10 %
6063-T5 12.7 mm (up to 0.500 in) 152 MPa (22.0 ksi) 110 MPa (16.0 ksi) 8 %
6063-T5 12.7 to 25.4 mm (0.501 to 1.000 in) 145 MPa (21.0 ksi) 103 MPa (15.0 ksi) 8 %
6063-T6 3.1 mm (up to 0.124 in) 207 MPa (30.0 ksi) 172 MPa (25.0 ksi) 8 %
6063-T6 3.2 to 25.4 mm (0.125 to 1.000 in) 207 MPa (30.0 ksi) 172 MPa (25.0 ksi) 10 %
6005A-T61 up to 0.249 in 262 MPa (38.0 ksi) 241 MPa (35.0 ksi) 8 %
6082-T6, T6511 5.1 to 19.1 mm (0.200 to 0.750 in) 310 MPa (45.0 ksi) 262 MPa (38.0 ksi) 6 %
6082-T6, T6511 19.1 to 152 mm (0.751 to 6.000 in) 310 MPa (45.0 ksi) 262 MPa (38.0 ksi) 8 %

Elongation is measured over a 50 mm (2 in) gauge length or 4 diameters, per the table’s heading. The values are minimums for an individual test, which is the sense in which the certificate quotes them.

The thickness bands differ by alloy. Writing the alloy, temper and the thickest wall on the order is what picks the row.

How the Limits Rise Across the Alloy Families

The same Association table spans the whole extrusion range, which lets a buyer place an alloy by its guaranteed strength before reading anything else. A short ladder of minimum yield strengths, taken from the same table for thin to moderate walls, shows the spacing.

  • 6063-T6, up to 3.1 mm: 172 MPa (25.0 ksi) yield, 207 MPa (30.0 ksi) tensile.
  • 6061-T6, up to 6.3 mm: 241 MPa (35.0 ksi) yield, 262 MPa (38.0 ksi) tensile.
  • 6351-T6, up to 3.1 mm: 255 MPa (37.0 ksi) yield, 290 MPa (42.0 ksi) tensile.
  • 6082-T6, 5.1 to 19.1 mm: 262 MPa (38.0 ksi) yield, 310 MPa (45.0 ksi) tensile.
  • 7005-T53, up to 19.1 mm (0.750 in): 303 MPa (44.0 ksi) yield, 345 MPa (50.0 ksi) tensile.
  • 7075-T6, up to 6.3 mm: 483 MPa (70.0 ksi) yield, 538 MPa (78.0 ksi) tensile.

The ladder moves from a soft anodizing alloy at the bottom to a high-strength alloy at the top, and the elongation floor falls as the strength rises, from 8 to 10 % for 6061-T6 and 6351-T6 to 7 % for 7075-T6 at these thicknesses.

The table also carries limits that are maximums. Annealed 6061-O gives no minimum and sets a ceiling of 152 MPa (22.0 ksi) tensile and 110 MPa (16.0 ksi) yield with 16 % elongation. The 6063-T52 row gives both a floor and a ceiling, 152 to 207 MPa (22.0 to 30.0 ksi) tensile and 110 to 172 MPa (16.0 to 25.0 ksi) yield for sections up to 25.4 mm (1.000 in).

A maximum in a limit row is a request for a soft or a bounded material. A buyer who sees one on a drawing is looking at a request for a bounded material, and the reason for it is a question for the extruder.

A bounded row also changes how a certificate is read. Any tensile value above the ceiling of an O or T52 row fails the lot even though the same number would pass in T6.

Four conditions in the footnotes to the Association’s table decide how a row is used.

First, the thickness of the cross-section from which the tension specimen is taken determines which properties apply. Second, for profiles thinner than 1.6 mm (0.062 in) the elongation test is not required, which fits the catalog description’s statement that elongation requirements stop below specified size limits. Third, the properties of T6 and similar tempers can usually be obtained by the user who properly solution heat treats from the O or F temper, though a part that has been formed or worked may come out lower. Fourth, 6063-T52 is called a producer temper and an exception to the ANSI H35.1 designation paragraphs.

A lot certificate therefore speaks for the product as shipped. What the buyer’s own forming, straightening or heat treatment does to it is outside the number.

Stress-Relieved Tempers and the Word Agreed

The tolerance tables treat the stress-relieved tempers in two groups. Footnotes of the Association define TX510 and TX511 as general designations for them, and only the first group is left to agreement.

Table 3. Stress-relieved temper groups named in the footnotes to the Aluminum Association’s tolerance tables 11.5 to 11.14 (2009 reprint)
Group Tempers it names
TX510 T3510, T4510, T61510, T6510, T8510, T73510, T76510
TX511 T3511, T4511, T61511, T6511, T8511, T73511, T76511

A buyer who orders 6082-T6511, as the table above shows, is ordering into the second group, TX511, whose profile tolerances are printed. For the T3510, T4510, T6510, T73510, T76510 and T8510 tempers of the first group, the footnote leaves the values to be settled between purchaser and vendor when the order is placed.

What a Supplier Signs and What the Buyer Still Has to Write

A certificate that cites B221 is a statement about composition and tensile behavior. The list below sets the statement against what a drawing still has to carry.

  • The alloy and temper, written in ANSI H35.1 form, for example 6061-T6 or 6063-T5.
  • The edition of B221 or B221M, since the standard is revised, and the catalog page shows B221-21 as the active revision.
  • The thickness band that governs, because the elongation row and, for 6063-T5, the strength row change with the thickest wall.
  • The dimensional standard for the profile geometry, which B221 does not supply. The Aluminum Association’s tolerances in ANSI H35.2 are the usual companion, and the piece on that standard in these resources reads its tables.
  • Any requirement for pressure service, which sends the part to B210, B241 or B234 and not to B221.
  • The units, inch-pound under B221 or metric under B221M.

A supplier signs the certificate to the standard. Whether the parts then fit depends on the other items in the list, which the standard leaves to the buyer.

Reading a Mill Certificate Against B221

A mill test report for an extruded lot normally lists the heat, the alloy and temper, the chemistry and the measured tensile, yield and elongation. Four checks apply.

  1. The alloy and temper on the report match the order line, character for character.
  2. The measured tensile and yield exceed the table minimums for the thickness band of the lot, and the elongation meets its row.
  3. The chemistry sits inside the limits for the alloy.
  4. The report names the specification and its edition.

The catalog description says samples are taken from ingots or from finished products. A certificate can therefore rest on a test of the ingot, of the finished product or of both, and a buyer who needs the finished-product value asks the supplier which one the report shows.

Because the limits are minimums for individual tests, a measured value far above the minimum is not a defect. Neither does it mean the profile is a better alloy, and a buyer who sees 6063-T6 at 228 MPa (33 ksi) has the same alloy as one who sees 207 MPa (30 ksi).

The catalog page says elongation requirements do not apply below specified size limits. For a thin-walled profile that means no elongation limit may apply, which is a feature of the standard and not an omission by the mill.

One 14 mm Wall Read Under Two Systems

A 6063-T5 profile with a 14 mm (0.55 in) wall shows how the same part meets two sets of limits. In the Association’s table the wall falls in the 0.501 to 1.000 in row, which gives 145 MPa (21.0 ksi) tensile and 103 MPa (15.0 ksi) yield with 8 % elongation. Hydro’s EN 755-2 table places it in the 10 to 25 mm band, which gives 160 MPa tensile and 110 MPa yield with 7 % elongation.

The yield figures sit 7 MPa apart and the tensile figures 15 MPa apart, with the European limit higher on both and the elongation floor 1 point lower. Neither figure is wrong, and a lot that meets one may or may not meet the other.

A supplier who certifies to the North American limits and a customer whose inspection plan is written to EN 755-2 can therefore disagree about the same lot without either of them making an error. The cure is on the purchase order: name one standard, and when a customer needs both, ask the extruder to confirm in writing that the lot is tested to the stricter row of each.

The 14 mm wall is a boundary case only because the two tables break at different thicknesses. A part that sits in the thick band of one and the thin band of the other needs the order to say which table governs.

Where B221 Stops and the Other Documents Start

The same profile is described by three kinds of document, and a clear order separates them.

Material belongs to B221 or B221M, with alloy and temper by ANSI H35.1. Geometry belongs to the dimensional tolerance tables, usually the Aluminum Association’s ANSI H35.2 and, for European supply, EN 755-9 or EN 12020-2. Surface belongs to the finish standard for anodizing or coating, a separate document.

A European reader will note that the same alloys appear in Hydro’s EN 755-2 sheets with limits in MPa, in thickness bands of millimeters, and with different band edges. The 6063-T6 minimum yield is 170 MPa up to 10 mm there and 172 MPa up to 3.1 mm in the table above, and the two sets are not interchangeable. One of them has to govern the certificate.

When a drawing is written in inches and a few hundred lengths are wanted before a production die is justified, low-volume profile extrusion and bridge production are the two places to ask which edition and which units the first run will be certified to.

Sources and Further Reading

Send the Section Drawing of Your Profile

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Profile Extrusion chosen.

Request a Quote