Test panels for AAMA 2605 sit on a fence in South Florida, south of latitude 27° N, tilted 45° to face the sun, for at least ten years. A coating that passes comes back with its color within 5 ΔE of where it started, a chalk rating of 8 or better and half its gloss still there. Qualicoat’s top class sends its panels to the same state for the same decade. The two systems, one North American and one European, reach a painted extrusion through different kinds of paperwork, yet both end at the same Florida test fence.
For a buyer, the practical question is narrower. Which class or tier goes on the drawing, what a coater or paint maker signs to claim it, and what the specification still leaves to be agreed? The answers sit in the comparison tables published by the Powder Coating Institute, in Qualicoat’s own introduction to its specifications, in coating makers’ guide specifications, and in the AAMA 605-98 text that preceded the current AAMA family.
What Qualicoat and AAMA 2603, 2604 and 2605 Cover
Qualicoat is a quality label for coatings on aluminum for architectural use. Its 26th edition, introduced in the document QCT-INTRO-26 valid from 1 January 2026, splits the specifications into three volumes: one for coaters, one for makers of chemical pretreatments and one for powder makers. Volume 1 sets minimum requirements that a production site, its coating lines, processes and finished products meet before a licence is granted to a coating plant. The full volumes are supplied on written request, and the introduction is the openly published part.
The AAMA documents, now issued through FGIA, are voluntary specifications for organic coatings on aluminum extrusions and panels. Sherwin-Williams’ guide specification section 050513 cites them by full title and 2022 edition:
- AAMA 2603, pigmented organic coatings;
- AAMA 2604, high performance organic coatings;
- AAMA 2605, superior performing organic coatings.
A course published by BNP Media describes the three as good, better and best, matched to one, five and ten years of color retention and chalk resistance. It adds that the older AAMA 603 and 605 were superseded by this family. The 1998 text of AAMA 605, published openly by Public.Resource.Org, shows the structure that carried over: a scope limited to factory-applied spray coatings, a definition of exposed surfaces as those the architectural drawings show visible when installed, and a test list from color uniformity to weathering.
Qualicoat certifies a coating plant and the products it approves. AAMA 2603 to 2605 define test results a coating system and its application have to reach. A drawing can call either, but it needs to name one.
Qualicoat Classes and AAMA Tiers Side by Side
The Powder Coating Institute’s comparison chart, updated March 2021, places Qualicoat Classes 1, 2 and 3 beside FGIA AAMA 2603-21, 2604-21 and 2605-20. Its Qualicoat column predates the 26th edition, and the class figures below are as the chart prints them.
| Requirement | Qualicoat Class 1 | Qualicoat Class 2 | Qualicoat Class 3 | AAMA 2603-21 | AAMA 2604-21 | AAMA 2605-20 |
|---|---|---|---|---|---|---|
| Minimum film | 60 µm (2.4 mil) powder | 60 µm (2.4 mil) powder | 50 µm (2.0 mil) powder | 20 µm (0.8 mil) | 30 µm (1.2 mil) | 30 µm (1.2 mil) |
| Humidity | 1,000 h, ISO 6270-2 | 1,000 h | 2,000 h | 1,500 h, ASTM D4585 | 3,000 h | 4,000 h |
| Salt spray | 1,000 h acetic, ISO 9227 | 1,000 h acetic | 2,000 h acetic | 1,000 h, ASTM G85 | 1,500 h | 2,000 h |
| Florida exposure | 1 year | 3 years | 10 years | 1 year | 5 years | 10 years |
| Gloss retention after Florida | 50 % | 50 % after year 3 | 50 % after year 10 | no checking, crazing or adhesion loss | 30 % | 50 % |
| Color change after Florida | ΔE 2 to 8 by color | ΔE 2 to 6 by color | ΔE 3 to 5 by color | slight fading allowed | under 5 Hunter units | 5 ΔE, PPG |
The chart also lists the laboratory tests behind the classes. On the Qualicoat side these are Buchholz hardness of at least 80 to ISO 2815, cross-cut adhesion to ISO 2409 at class Gt 0, cupping of at least 5 mm to ISO 1520, a mandrel bend of 5 or 8 mm to ISO 1519 and an impact of 2.5 N·m (22 in·lb) to ASTM D2794. Qualicoat also runs a Machu test of 48 h at 37 °C (99 °F) with no more than 0.5 mm (0.02 in) creep at the cross cut and a Kesternich sulfur dioxide test of 24 cycles.
The AAMA side uses ASTM methods. Pencil hardness to ASTM D3363 is listed at H, cross-cut adhesion to ASTM D3359 with no loss, and wet and boiling water adhesion repeat that test after 24 h in water at 38 °C (100 °F) and after 20 minutes in boiling water. AAMA adds chemical resistance with muriatic acid, mortar, detergent and window cleaner for all three tiers, plus nitric acid and falling-sand abrasion for 2604 and 2605. The abrasion figure doubles from 40 L of sand for 2604 to 80 L for 2605.
One difference matters on the shop floor. The PCI chart records that Qualicoat expects the coating not to crack or chip when the coated part is sawn, milled or drilled with sharp tools. AAMA’s tier tables have no such row, so a painted extrusion that will be machined after coating is better served by a requirement written into the order.
Film Thickness on an Extrusion and Where It Falls Short
Each tier’s thickness is a minimum on the faces that matter, not an average over the whole profile. AAMA 605-98 spelled out the rule its successors grew from: the total dry film is at least 1.2 mil (30 µm) on significant exposed surfaces, 80 % of readings meet or exceed it, and no reading falls below 1.0 mil (25 µm) or 85 % of the specified thickness. A note in the same clause concedes that the shape of an extrusion can defeat the spray gun. Inside corners and channels may not reach the minimum, and the text tells the buyer to settle those areas with the applicator before painting.
Coating makers publish the film builds they intend. Table 2 shows the dry film thickness ranges in Sherwin-Williams’ guide specification for extrusion coatings, measured to ASTM D7091.
| AAMA tier and resin | Primer | Color coat | Total |
|---|---|---|---|
| 2605, 70 % PVDF, two-coat | 5 to 13 µm (0.20 to 0.50 mil) | 25 to 38 µm (1.00 to 1.50 mil) | 30 to 51 µm (1.20 to 2.00 mil) |
| 2605, 70 % PVDF with clear topcoat | 5 to 13 µm (0.20 to 0.50 mil) | 25 to 51 µm (1.00 to 2.00 mil) | 38 to 76 µm (1.50 to 3.00 mil) |
| 2604, 50 % PVDF | 5 to 10 µm (0.20 to 0.40 mil) | 25 to 43 µm (1.00 to 1.70 mil) | 30 to 48 µm (1.20 to 1.90 mil) |
| 2604, super durable polyester | 5 to 10 µm (0.20 to 0.40 mil) | 25 to 30 µm (1.00 to 1.20 mil) | 30 to 41 µm (1.20 to 1.60 mil) |
| 2603, acrylic and polyester one-coat | none | 20 to 36 µm (0.80 to 1.40 mil) | 20 to 36 µm (0.80 to 1.40 mil) |
The table shows how resin and tier are tied. That guide specification describes its 2605 extrusion coatings as containing at least 70 % PVDF resin by weight in the color coat, and its 2604 fluoropolymer as at least 50 %. BNP’s course gives the same split by chemistry: polyester and acrylic for 2603, silicon polyester for 2604 and 70 % PVDF for 2605. PPG’s description of its 2605 coatings names FEVE resin systems as a second chemistry that meets the tier.
Powder runs thicker. The PCI chart lists Qualicoat minimums of 60 µm (2.4 mil) for powder in Classes 1 and 2 and 50 µm (2.0 mil) in Class 3, measured by eddy current to ISO 2360. The AAMA tiers, by contrast, state their minimums for the whole film, primer and color coats together where both are used.
The thickness on the drawing applies to the exposed faces. Channels and inside corners need their own line on the drawing, or they will be argued over after painting.
Pretreatment Under the Paint
Every tier rests on the chemistry applied before the paint. AAMA 605-98 described a multi-stage cleaning and pretreatment system that removes soils and residual oxide and leaves a conversion coating to which the organic coating bonds, with a minimum conversion coating weight of 30 mg/ft2 (323 mg/m2). The PCI chart carries this forward: 2604 lists a chromate conversion above 323 mg/m2 measured to ASTM D5723, and 2605 lists an amorphous chromium phosphate treatment to ASTM D1730 above 430 mg/m2, with alternative chrome and non-chrome conversion coatings permitted if they meet the performance requirements.
Qualicoat treats pretreatment as its own approval. The 26th edition introduction defines approval categories, among them A-No. for a chemical pretreatment on etched material and AP-No. for one on pre-anodized material. Volume 2 sets the approval procedure for pretreatment makers, including outdoor exposure in Genoa. Its Volume 1 lists surface preparation, chemical conversion and pre-anodizing among the work specifications a coater follows, and the introduction names three endorsements a licensee can hold:
- SEASIDE, for coastal exposure.
- PRE-OX, for pre-anodizing as the pretreatment.
- POSTFORMING, for coated sheet that is bent or stamped after coating.
Alumil, a Greek extruder and coater, describes what the seaside class means on its line: a chemical pretreatment with an etching degree of at least 2.0 g/m2, which it attributes to Qualicoat and GSB requirements for seaside class profiles. It offers pre-anodizing as an option against filiform corrosion for projects near the coast or swimming pools. Qualicoat’s standards list includes ISO 4623-2 for filiform corrosion on aluminum, the test that checks this. The same coating line often carries the flat panels an extrusion frame holds, cut from sheet by laser cutting and bent, so a frame and its panels can be pretreated and coated together to one approved color.
Color, Gloss and the Approved Sample
Neither system sets one color tolerance for every color. The PCI chart records that Qualicoat qualifies coatings on three colors chosen by its committee, while the AAMA tiers require color consistent with an established range. AAMA 605-98 gave the method: random samples checked visually under a uniform light source such as a MacBeth daylight lamp or the north sky, viewed head-on, and judged against a range agreed between the approval source and the applicator.
The same 1998 clause added a practical caution that still applies. Color and finish can vary with spray equipment, line conditions and day-to-day process changes, and the text strongly recommends that final color approval limits come from production line samples or mock-ups rather than laboratory panels. Metallic, mica and pearlescent finishes need tighter control because flake orientation affects color uniformity.
Gloss has numbers. AAMA allows ±5 units of the coating maker’s specification on a 60° gloss meter to ASTM D523, and AAMA 605-98 gave reference bands of 80 and over for high gloss, 20 to 79 for medium and 19 or less for low. The PCI chart shows Qualicoat with a tolerance that widens with the gloss level, ±5 units from 0 to 30, ±7 from 31 to 70 and ±10 from 71 to 100, measured to ISO 2813.
| Item | Qualicoat, as compared by PCI and its standards list | AAMA 2603 to 2605 and AAMA 605-98 |
|---|---|---|
| Gloss method | ISO 2813 | ASTM D523, 60° |
| Gloss tolerance | ±5 (0 to 30), ±7 (31 to 70), ±10 (71 to 100) | ±5 units of the maker’s value |
| Color method | ISO 11664-4, CIE 1976 Lab* | visual under uniform light; instrument values agreed |
| Color reference | three committee colors for approval | range agreed between approval source and applicator |
| Color after weathering | ΔE limits by class and color | Hunter units or ΔE by tier |
Sherwin-Williams’ guide specification shows how the agreement reaches paper. It asks for two samples of 3 × 3 in (76 × 76 mm) for each color, gloss and substrate, and its applicator warranty treats fading of more than 5 ΔE Hunter units to ASTM D2244 and chalking beyond No. 8 to ASTM D4214 as deterioration.
Weathering Proof in Florida and the Cabinet
Florida exposure separates the tiers more than any laboratory test. AAMA 2603 calls for one year, which the BNP course describes as optional and PPG describes as about one year; 2604 calls for five; 2605 for ten.
The BNP course sets the chalk limit after ten years at No. 8 for colors and No. 6 for whites, on a ten-point scale where higher is better.
Qualicoat grades its classes the same way. Class 1 is exposed in Florida for one year at 5° facing south, Class 2 for three years, and Class 3 for ten years at 45°, with gloss retention checked along the way. For Class 3 the PCI chart lists 80 % gloss retention in the third year, 55 % in the seventh and 50 % in the tenth. Classes 1 and 2 also take 1,000 h in a xenon arc cabinet, with 50 % and 90 % gloss retention respectively; for Class 3 that cabinet test is replaced by the Florida results.
A ten-year test means a coating approved today was formulated and panelled a decade ago. Approval belongs to the coating system, which is why the AAMA guide specification asks for test reports showing conformance, and why a Qualicoat label points to an approved powder, an approved pretreatment and a licensed plant together.
What a Supplier Signs and What the Standards Leave Open
What changes hands is a set of documents, not a single certificate. Drawn from the sources above, a complete submission for a coated extrusion usually holds:
- the coating maker’s product data, naming the AAMA tier or the Qualicoat approval number of the system;
- test reports for the tier, including Florida exposure results;
- the coater’s Qualicoat licence and any SEASIDE or PRE-OX endorsement, where Qualicoat is specified;
- color and gloss samples from the production line, signed as the approved standard;
- the dry film thickness range for each coat, and the warranty terms for color change and chalk.
Several points stay open unless the order closes them.
The thickness in channels and inside corners, which AAMA 605-98 left to the applicator, is one. Sealant compatibility is another: the 1998 text required sealants compatible with the coating and pointed fabricators to their sealant supplier. Touch-up is a third, where repairs were to match color and gloss and pass dry adhesion after 72 h. Machining after coating, covered by Qualicoat’s tool test and absent from the AAMA tier tables, is a fourth.
First production lengths are where those open points are settled, on real profiles rather than flat panels. When a coated profile needs its first lots approved for film, color and gloss before volume, low-volume profile extrusion and bridge production are where the tier, the approved sample and the channel thickness are agreed before the first rack is coated.
Sources and Further Reading
- PCI Architectural Specification Comparison, updated March 2021, Powder Coating Institute
- Introduction to the QUALICOAT Specifications, 26th Edition, QCT-INTRO-26, valid from 2026-01-01, QUALICOAT
- AAMA 605-98, Voluntary Specification, Performance Requirements and Test Procedures for High Performance Organic Coatings on Aluminum Extrusions and Panels, American Architectural Manufacturers Association, published by Public.Resource.Org
- Section 050513, Factory-Applied (Baked On) Coatings for Metal, guide specification, Sherwin-Williams
- FGIA/AAMA 2605, High Performance and Monumental, PPG
- FGIA/AAMA 2603, Residential and Interior, PPG
- AAMA 2605-05 Sets High Standards for Coated Aluminum Extrusions and Panels, BNP Media Continuing Education Center
- Powder Coating for aluminum extrusion, Alumil