DrawingCross-SectionWall Thickness

Aluminum Extrusion Die Design and the Die Trial Before the First Billet

A die is balanced, strengthened and simulated before steel is cut, and the first trial proves the flow, the walls and the visible faces.

A two-part steel extrusion die for a hollow profile taken apart, the mandrel with its ports beside the die plate, with the first short trial pieces of the hollow aluminum profile.

In the first design of a porthole die studied by Liu and colleagues, metal left one end of the opening at 182.3 mm/s (7.18 in/s) and the other at 111.0 mm/s (4.37 in/s). The profile was 107.57 mm (4.24 in) long in section, with a small 4.04 mm (0.16 in) cavity at one end, and the fast side pushed the slow side until the bar bent. Three design changes later, the spread across the same section was 2 mm/s (0.08 in/s), and the die that went to the press produced straight lengths with a wall only 0.1 mm (0.004 in) from the drawing at the hard end.

That gap between a first drawing and a balanced die is what die design is for. A buyer never sees the die, but every straightness, wall and surface figure on the first lengths was set there before the first billet was heated. This article walks the design in the order a die maker follows and shows what the first trial is meant to prove.

From Drawing to Die in Six Steps

Hydro, which designs and builds extrusion dies in-house and with independent toolmakers, publishes its sequence for a custom die. Each step has a stated purpose:

  1. Consult: review the drawings, the alloy, the press size and the production volumes.
  2. Design: CAD die design, cavity strategy, press plan and expected productivity.
  3. Simulate: flow and temperature modelling to pre-balance the metal distribution.
  4. Manufacture: precision machining of the die, then heat and surface treatment.
  5. Control: first-article checks, with die correction as needed.
  6. Validate: confirm dimensional stability and surface finish, and document the optimal settings for the next production run.

Hydro states its aim as a die that reaches the tolerance targets on the first production run, and it lists the means: CAD modelling, flow simulation and experience on the press. Correction is part of the plan rather than an accident. It is described as iterative tuning, where needed, based on trial extrusion data, to meet the agreed tolerance and surface finish targets.

The Aluminum Extruders Council adds the condition that makes the sequence work. Its view is that the best combination of product performance and quality comes when the product designer, the die maker, the extruder and the purchaser recognize each other’s requirements and work together.

The die trial is the fifth step of six. By the time the first billet is pushed, the drawing, the alloy, the cavity count and the flow balance have already been decided.

Reading the Profile Before the Die Is Drawn

The die maker’s first job is to judge how hard the shape will be to extrude. Published guidelines from the Aluminum Extruders Council support that judgment, and several carry numbers.

Table 1. Profile design guidelines published by the Aluminum Extruders Council
Guideline Published value or rule Why it matters to the die
Circumscribing circle diameter most common profiles under 305 mm (12 in); a few extruders to 813 mm (32 in) a press’s capacity sets how large a profile it can produce
Economical range CCD of 25 to 254 mm (1 to 10 in); design enhanced under 203 mm (8 in) the council’s range for the most economical profiles
Weight per foot design enhanced at 4.5 kg/m (3 lb/ft) or less press operation and press size
Outside corners at least 0.51 mm (0.020 in) radius knife edges avoided by rounding
Inside corners at least 0.38 mm (0.015 in) radius where a sharp corner is needed, a corner relief is suggested
Wall thickness keep uniform; generous radius at thick-thin junctions thick-thin junctions cause distortion, die breakage and surface defects
Voids and tongues keep voids symmetrical; avoid high tongue ratios an asymmetric void raises the chance the die tongue breaks
Wide thin sections add ribs, webs or grooves ribs help straightening, reduce twist and improve flatness

The council presents these as guidelines to optimize process efficiency, not as limits. Complex profiles that break many of them are possible, it notes, and may be the right answer; the point is to discuss them with an extruder before the die is drawn.

Hydro’s list of what makes a die more demanding repeats the same features from the die maker’s side: critical cross-sections with tight tolerances, deep channels and high tongue ratios, varying wall thicknesses and a high surface finish all need more design time and more precise machining. Harder alloys and higher extrusion ratios generate more heat and wear, which may call for a higher grade of tool steel, nitrogen cooling or extra surface treatment.

Choosing the Die Class and the Number of Openings

The die itself is a steel disk, normally H13 tool steel according to the council, with the profile’s shape cut through it. Dies fall into two broad classes. A solid or flat die forms solid shapes, and it may have one opening or several.

Hydro adds that dies are machined from hardened tool steels chosen for wear resistance and thermal stability, with the grade set by the alloy being extruded and the expected production volume, and that nitriding or CVD coatings extend their life. Hollow dies form hollow and semi-hollow shapes with a mandrel held inside the opening, and the council names bridge, porthole and spider dies as its forms. It calls the porthole and pancake types the most common, the easiest to manufacture and the easiest to machine by CNC, which also lets the die maker and the die corrector quantify each alteration for future dies.

Hydro’s description of the hollow die explains where weld lines come from. The mandrel that forms the inside of the profile sits on a bridge; aluminum flows around the bridge and re-welds behind it before leaving the die. Hollow dies are more complex to design and make, which shows in their lead time.

Nor does the die work alone. The council describes a die assembly in which the die and a backer sit inside a die ring, placed in front of a bolster with a sub-bolster behind, all held together by a tool carrier. Backer and bolsters support the die against the extrusion load, and the council notes that, depending on the complexity of the shape, the tooling for a profile may include these supplemental tools as well as the die itself.

The number of openings is a design decision with a production reason. Hydro runs large and medium profiles through a single-cavity die to control flow and hold tight tolerances, and small profiles through multi-cavity dies with up to 16 openings. The reason is the minimum exit weight of the press line: a very small, light profile run alone is below the weight per meter the line handles well, and several strands together raise it. Hydro’s engineers set the cavity count from press tonnage, alloy, geometry and downstream handling, then balance the flow across the openings.

One opening gives the most control over a large profile. Several openings bring a light profile up to the weight the press line needs, and each opening then has to flow like the others.

Balancing Metal Flow at the Bearing

The council states the central rule of die design in one sentence: the effective bearing length controls the metal flow through the die, and the objective is to have all parts of the profile emerge at the same speed. A longer bearing adds resistance and a shorter one removes it, so thick parts of a profile are slowed with longer bearings to match thin parts with shorter ones.

The Liu study, published in Materials in 2018, shows how much work that rule can take on a difficult section. Its profile had a length to width ratio of 42.6, a minimum wall of 2.525 mm (0.099 in) and a small cavity at one end. The first die, with four symmetrical portholes and an 18 mm (0.71 in) welding chamber in the lower die, gave a standard deviation of exit velocity of 19.63 mm/s (0.77 in/s), and the profile bent along its length. Its authors then changed the die in three steps.

Table 2. Three die design changes and their effect, porthole die study for AA6063, Liu et al. 2018
Step Change to the die Measured effect in simulation
Initial design four portholes, welding chamber 18 mm (0.71 in) in the lower die maximum 182.3 mm/s, minimum 111.0 mm/s, deviation 19.63 mm/s
1 welding chamber moved to the upper die, port bridges sunk 24 mm (0.94 in), chamber height 15 mm (0.59 in), porthole entrance angle 30° maximum velocity down to 172.8 mm/s (6.80 in/s)
2 baffle plates added to feed the small cavity side, at a distance of 57.5 mm (2.26 in) near-uniform exit; at 55 mm (2.17 in) the solid end still ran fast and bent
3 bearing lengths adjusted in five regions, longer where metal ran fast velocity spread 7.71 to 2 mm/s (0.30 to 0.08 in/s); deviation 0.927 to 0.448 mm/s; distortion basically eliminated

The baffle step shows how sensitive the balance is. Moving the plates by 2.5 mm (0.1 in) took the profile from a severe bend at the solid end to a near-uniform exit, and moving them further made the cavity side run fast instead. Bearing adjustment then did the fine work, exactly as the council’s rule describes.

The die opening was also cut slightly oversize. They enlarged the orifice 1.01 times the drawing size to allow for shrinkage as the profile cools, and added a run-out behind the bearing so the emerging profile would not be scratched.

Die Strength, Deflection and Extrusion Load

A balanced flow is worth little if the die bends under load. In the Liu study, the small mandrel that formed the 4.04 mm cavity stood 26 mm (1.02 in) proud of the die surface and was supported by port bridges 26 and 18 mm (1.02 and 0.71 in) wide. The first design deflected 0.107 mm (0.0042 in) at the bridges and 0.0925 mm (0.0036 in) at the mandrel tip. Its designers judged the mandrel liable to bend or break in use, during splitting of the die or in transport, and did not use that design.

After the three changes, the upper die deflected 0.05945 mm (0.0023 in) and the mandrel 0.04648 mm (0.0018 in), small enough that the authors expected the deflection not to affect the profile’s dimensions. Balance came with more load. Baffles add resistance in the welding chamber, and the simulated load rose from 10,617.3 kN (about 1,190 US tons-force) to 13,903.2 kN (about 1,560 US tons-force). That was still within the 2,000 ton press used for the trial, and the authors note that too high a load causes intolerable wear, the major cause of die failure.

Temperature is checked at the same stage. The authors set 560 °C (1,040 °F) as the critical exit temperature for AA6063, above which hot tears and low properties follow, and the optimized die reached a maximum of 539.3 °C (1,003 °F).

Simulating the Die Before Steel Is Cut

Hydro’s third step, simulation, is where flow and temperature are pre-balanced before machining. The Liu study shows what a simulation needs to be trusted: the same process conditions the press will run, a flow stress law for the alloy measured on a thermomechanical simulator between 400 and 520 °C (752 and 968 °F), and friction and heat transfer assumptions at every contact.

Table 3. Inputs used to simulate the porthole die, Liu et al. 2018
Input Value
Container diameter 210 mm (8.3 in)
Billet length 350 mm (13.8 in)
Extrusion ratio 75.8
Ram speed 2 mm/s (0.08 in/s)
Billet temperature 480 °C (896 °F)
Container and die temperature 430 °C (806 °F)
Friction, billet to container and die sticking
Friction, billet to bearing sliding, coefficient 0.3
Heat transfer, billet to tooling 3,000 W/(m2·°C) (528 BTU/(h·ft2·°F))

For comparison, the Aluminum Extruders Council gives the general billet range as above 375 °C (700 °F) and up to 500 °C (930 °F), depending on alloy, and press capacities from 100 to 15,000 tons. The International Aluminium Institute adds that computer-aided design and manufacture shorten design time and improve tolerances. The die itself is machined steel that is cut and wire-eroded to the bearing lengths the simulation sets, which is why a change found after steel is cut costs a new die or a correction at the bearing rather than an edit to a file.

What the First Die Trial Shows

The trial is Hydro’s fifth and sixth steps: first-article checks with correction as needed, then validation of dimensional stability and surface finish against the agreed tolerances, with the optimal settings documented for the next production run. Liu and colleagues ran their trial the same way, on a real die in a 2,000 ton press with the simulated parameters. After drawing, straightening and correction, no distinct bend or twist was found along the length, the wall at the small cavity was within 0.1 mm (0.004 in) of the requirement, and micrographs showed no sign of overheating.

The first lengths also reveal what the design fixed for good. A KFUPM study of extrusion defects lists several that trace back to the die:

  • weld lines, which die design can place on faces that are not seen in the finished product;
  • die lines, reduced by a minimum choked land length and a polished land;
  • black lines from local high pressure in the welding chamber, often visible only after etching;
  • bending and twisting in multi-hole dies, prevented by centering the cavities for equal flow;
  • uneven wall in a hollow, caused by a mandrel that is not centered.

Hydro notes that correction after trial runs is sometimes needed, particularly for complex or critical profiles, to reach the final drawing. Because porthole and pancake dies are cut by CNC, the council observes, each correction can be quantified and carried into future dies.

What the Buyer Brings to the Die Design

Hydro’s first step lists what the die maker needs from the buyer: the drawing, the alloy, the press size and the production volumes. The defects and guidelines above add a few items worth placing on the drawing or in the order: which faces are visible, so welds and die lines can be kept off them; which dimensions are critical, so the bearing balance can favor them; and whether the profile will be anodized, since some die-related marks show only after etching.

The first trial is where those choices are proven on metal. When a new profile needs its die designed, trialed and corrected before volume, low-volume profile extrusion and bridge production are where the visible faces, the critical dimensions and the first-article checks are agreed before the first billet is pushed.

Sources and Further Reading

Send the Section Drawing of Your Profile

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Profile Extrusion chosen.