Hollow Profile6063Sample

Aluminum Extrusion Process From Billet to Aged Profile

The press pushes a softened billet through a die, and the quench, stretch and oven that follow decide whether the bar is straight and strong.

The stages of aluminum extrusion side by side, a short round billet, a raw extruded profile length and a finished anodized length.

A 6063 profile has to leave the die at 499 °C (930 °F) or hotter, measured at the press platen, and yet it has to be cool enough to grip and pull straight a few dozen meters later. One extruder’s process sheet gives that exit figure for 6063, 6463, 6063A and 6101, and a slightly higher 510 °C (950 °F) for 6005A and 6061. Between the die and the stretcher jaws the metal travels a run-out table that runs 30 to 40 m, cooling as it goes, and much of what a buyer later measures as bow, twist or hardness is decided on that table or in the minutes before it.

The sequence looks short on paper: heat a log, push it through a steel plate, cool it, stretch it, cut it, age it. Each of those verbs carries a temperature, a percentage or a length that published sources print, and each one has a failure that shows up as a mark on the surface or a bend in the bar. The walk below follows the metal in the order it meets the equipment.

The Steps of Aluminum Extrusion in the Order the Metal Meets Them

Seven operations turn a cast billet into a profile ready for finishing. A billet is a solid cylinder of cast aluminum, and it never melts on the way. It is softened in a furnace, loaded into a container, and squeezed through a die by a hydraulic ram, with the fraction of metal near the die face discarded at the end of every push.

Table 1. The operations from billet to aged profile, with the figures published for each
Step Operation Published figure Source
1 Heat the billet in a gas furnace or an induction heater about 427 to 496 °C (800 to 925 °F); up to 500 °C by alloy Alliance process sheet; Aluminum Extruders Council (AEC)
2 Load, lubricate the billet and ram, push the dummy block thin film of lubricant on billet and ram Alliance process sheet
3 Upset against the die, then extrude billet shortens and widens until it fills the container AEC process page
4 Shear off the butt, load the next billet butt of about 10 % of billet length (12 to 14 % of billet weight in one allowance) Illinois thesis; Light Metal Age
5 Quench on the run-out table air, mist, water spray or water bath AEC Aluminum Extrusion Manual
6 Stretch, then saw to length stretch of 1 to 3 % Illinois thesis
7 Age in an oven 165 to 195 °C range plotted on an alloy datasheet Hydro 6063 datasheet

Read down the figures and a pattern appears. Getting metal to flow at the right temperature and pressure takes up the first four steps. Straightness and strength come from the last three. At the junction sits the die, and the discard in step 4 is the price of keeping the skin of the billet out of the profile.

Three questions sort most of what follows in the walk:

  • Which temperature is being quoted, and is it read at the billet, the platen or the die.
  • Which part of the push the sample came from: front end, steady state or butt side.
  • Which treatment came after the press: stretch percentage, quench method and temper.

A profile is shaped in seconds at the die, but its straightness and its strength are fixed afterward, by the quench, the stretch and the oven.

The Dummy Block and the Container Wall

In the arrangement the Alliance sheet draws, the ram pushes a dummy block, the dummy block pushes the billet, and the billet is forced through a die held in a stack of support tooling. A thin film of lubricant on the billet and ram keeps the two from sticking. One source on billet geometry explains that metal near the liner wall flows differently from metal at the center, and that the die designer has to account for it wherever ports or pockets approach the wall.

Billet Heating and the Temperature Window

The billet comes out of casting at room temperature and enters the press at a temperature that depends on the alloy. For the 6xxx family, which covers most architectural and industrial profiles, one extruder’s sheet gives a billet range of about 427 to 496 °C. The Aluminum Extruders Council describes a typical range as above 375 °C and up to 500 °C depending on the alloy. Both sit far below the melting range of 6063, which a producer datasheet gives as 615 to 655 °C.

A gas furnace and an induction heater do the same job at different speeds. According to a University of Illinois thesis on extrusion modeling, an induction coil holding three or four billets runs a continuous cycle, with 3 to 20 minutes between loading a billet and removing it, and that a high-speed gas furnace takes three to five times longer for the same heating. Few buyers ask which one a plant uses, yet the difference explains why one press can change billets quickly and another cannot.

Why the Container Runs Cooler Than the Billet

Heat is not only something the furnace adds. Friction against the liner and the work of squeezing the metal both warm it as the stroke runs, so a billet that starts at its target temperature can finish the push several degrees hotter. A Light Metal Age article on billet geometry reports modeling in which a container held at least 50 °F (about 28 °C) cooler than the billet gave better productivity and reduced how much skin flowed into the profile. The same article suggests that a container with high-conductivity steel and cooling fans on the outside is the way to hold that difference.

The practical result for a buyer is a quiet one. A press that holds a controlled gap between billet and container temperature runs the same die at a more even speed, and an even speed gives an even surface.

Temperatures That Define the Window

Table 2. Temperatures named in the sources, by where they are measured
Where Temperature Alloy or condition Source
Billet entering the press 427 to 496 °C (800 to 925 °F) 6xxx family, per the process sheet Alliance process sheet
Billet, general range above 375 °C, up to 500 °C (930 °F) by alloy AEC process page
Press exit, at the platen 499 °C (930 °F) minimum 6063, 6463, 6063A, 6101 Alliance process sheet
Press exit, at the platen 510 °C (950 °F) minimum 6005A, 6061 Alliance process sheet
Inside the press, typical 482 to 593 °C (900 to 1,100 °F) 6xxx alloys AEC Aluminum Extrusion Manual
Container relative to billet at least 28 °C (50 °F) cooler modeled 8 in. and 10 in. billets Light Metal Age

The AEC manual adds a caution that matters when a number from one document meets a number from another: press exit temperatures are taken at the platen, and actual temperatures at the die exit are significantly higher. Two plants can quote different exit figures for the same alloy and both be right, because one reads at the platen and the other infers at the die.

The Press Stroke From Upset to Butt

With the billet in the container, the ram advances the dummy block and the billet is crushed against the die. It shortens and widens until it touches the container wall everywhere, a step the AEC calls upsetting. Pressure then rises, and the solid metal starts to squeeze through the die orifice.

Hollow Shapes and Where They Weld

A solid profile passes through a flat plate with a cavity cut to its outline. Hollow profiles need a core, and the core has to be held in place by something in the metal’s path. The AEC explains that the metal divides around a mandrel supported on bridges, then rejoins under pressure in a welding chamber before reaching the bearing. That rejoining leaves seam lines along the length of the bar. A well-run die and press make the weld sound, but it is a joint, and a buyer who plans to anodize, bend, or pressurize a hollow profile should know it exists.

Cooling the Die and Keeping Oxide Out

An Alliance process sheet describes liquid nitrogen flowing around parts of the die during the push, which both cools the tool and surrounds the emerging shape with an inert atmosphere that keeps oxide from forming on the surface. Some plants use nitrogen gas instead, which provides the atmosphere without cooling. The same sheet notes that the press records the exit temperature at the platen, mainly so the operator can hold the highest speed the alloy allows.

The Butt and the Billet Behind It

Stopping the push early leaves a disk of metal in the container. That butt carries the oxide-rich skin of the billet, and it is sheared off and recycled while the next billet is loaded. The Illinois thesis gives the usual butt thickness for direct extrusion as about 10 % of billet length. Light Metal Age states the standard allowance as 12 to 14 % of billet weight to keep skin and coring out of the profile, and it points out that longer billets produce longer butts, with a trade-off either way. Stop the push at 14 % and the butt is long and hard to shear cleanly; extrude down to a butt an inch or two thick and contamination collects in the die and in the back end of the bar.

Billet length itself has changed over time. The same article notes that containers once held billets about five times as long as they were wide, and that longer containers now allow up to eight times. Longer is not automatically faster. The authors’ modeling found nearly identical press load and die temperatures for an 8 in. by 56 in. billet and a 10 in. by 35.8 in. billet of similar weight.

The butt is not waste by accident. It is the part of the billet that cannot be trusted, and every push gives up between a tenth and a seventh of its weight to keep the profile clean.

Billet on Billet and the Puller

To make long continuous lengths, plants weld each billet to the one before it in the solid state. A feeder plate or pocket die in front of the die helps. The result is a profile that does not stop at each billet change, and the Illinois thesis describes a puller gripping the section as it leaves the press and guiding it down the run-out table in step with the ram. Because the puller stops automatically when the press stops, it is one reason a modern line can hold twist and surface better than hand-guided runs.

Quenching on the Run-Out Table

Cooling begins the instant the profile leaves the die, and its job is to hold the alloying elements in solution so the oven can precipitate them later. The AEC manual lists four methods: air, mist, water spray and water bath. Water spray, the Illinois thesis adds, is gradually replacing tank-type water quench and over-table fans, and that high-pressure sprays can cool difficult shapes quickly while limiting distortion.

Air is the gentlest method, and it is the one used for the heat-treatment data in Hydro’s 6063 datasheet, whose plotted aging curves start from a 200 by 3 mm solid profile air quenched after extrusion and held for 24 hours before artificial aging. The thesis adds that high-pressure sprays exist for shapes that are difficult to cool, and that they are used to limit distortion while reaching the cooling rate the alloy needs.

The Press Line Can Gain Speed From the Temperature Profile

A trade-journal article on billet quenching describes cooling the billet along a taper before the push, so that temperature stays even through the stroke and the ram does not have to slow near the end. It cites a 10 to 45 % expected increase in ram speed for the same die, and average press-speed gains of about 28 % across four dies in one case study. These are figures from an equipment supplier’s perspective, so treat them as an upper picture of what is possible rather than a promise for every profile.

Stretching, Sawing and Aging

After quenching and cooling, the bars are moved to a stretcher. Quenching leaves distortion and residual stress in the section, and a pull of 1 to 3 % straightens the bar and relieves much of that stress. The Illinois thesis notes that the stretcher has to exceed the force obtained by multiplying the cross-section area by the yield strength of the alloy, and that grip pressure has to be controlled so the jaws neither slip nor crush the section too far.

What the Stretcher Leaves at the Ends

The jaws leave marks. Roughly 1 m at each end is crushed or of low quality in the thesis’s accounting, so about 2 m per continuous length is lost, and the Alliance sheet adds that the ends of a bar are usually not to tolerance and are removed as scrap. Alliance describes a standard bar of about 18 ft (5.5 m) cut into the lengths each part number needs, which is why part lengths are planned inside the bar and not at its ends.

Sawing to Length

The stretched bars go to a saw table, where they are pushed against a gauge stop and cut. A high-speed circular saw trims the grip marks and the front and back ends, and it cuts the finished lengths. Saw chips are collected by a high-pressure vacuum, the thesis notes, and several extrusions can be cut at once, depending on the section, the alloy and the saw’s capacity. From the Alliance sheet comes a standard saw cutting tolerance of 0.125 in. (3.2 mm) or greater, depending on saw length, for an 18 ft standard bar. A buyer who needs a tighter cut length than that has the bar cut a second time on a precision saw.

Aging in an Oven

Aging is the last heat-treating step. Under EN 515, which Hydro’s 6063 datasheet cites, a T5 temper is cooled from a hot shaping process and then artificially aged, while a T6 temper is solution heat treated and then artificially aged. For 6xxx alloys the first stage of that sequence happens in the press itself, as the Illinois thesis explains: the press exit has to be hot enough that the metal is effectively solution treated, and the quench holds it that way. Aging then happens in separate ovens, often with racks moved by conveyors.

The datasheet plots how strength rises with aging time at 165, 175, 185 and 195 °C, which shows that time and temperature trade against each other. It does not print a single recipe, and neither do the other sources opened for this piece, so the exact hours belong to the extruder’s approved procedure for the alloy and temper, not to a buyer’s guess. What a buyer can check is the result: the same datasheet lists for 6063-T5 in sections up to 10 mm thick a minimum yield strength (Rp0.2) of 130 MPa and a minimum tensile strength of 175 MPa, with elongation of 8 %.

Table 3. What goes wrong at each step and how it is seen
Step What goes wrong How it is seen
Billet heating uneven temperature along or across the billet tearing or speed cracks at the surface; inconsistent speed
Extrusion die flow out of balance across the section bow, twist or a wall that runs thick on one side
Butt shear skin or oxide reaches the profile streaks or blisters near the back end of a push
Quench cooling too slow or uneven low hardness after aging; distortion toward the cooled side
Stretch grip slip or overstretch marks near the ends; a bar that springs back out of straight
Saw dull blade or poor support burr, out-of-square cut, chatter on thin walls
Aging wrong time or temperature for the temper hardness under the datasheet figure

The cause-and-symptom pairs in the table follow from the mechanics in the sources, but the sources do not rank them or give rates, so treat the list as a map of where to look and not as a frequency table.

What to Ask Before You Accept the Bar

An engineer reading a first-article report can tie most of the questions to the steps above. The temper comes first, with the section thickness it covers, because the minimum values in a datasheet are stated per thickness band. Where the sample bar sat in the push matters next, since the butt and the billet changeover are where variation concentrates. Stretching and squareness of the cut close the list.

  • The temper that was delivered, with the thickness band it was tested in.
  • Which part of the billet the sample came from, and whether the bar was in the middle of a continuous run.
  • Whether the press exit temperature or the quench method differs from the one used for the datasheet figures.
  • Whether stretching was applied, and what length of each bar end was removed.
  • Whether any part of the lot was cut from the end zones that the stretcher marks.

The answers say more about how repeatable the second lot will be than any single measurement does. A profile made at the same exit temperature, quenched the same way, stretched the same amount and aged to the same temper will measure the same, and a supplier who can state those four conditions is working to a procedure.

The numbers that matter to a buyer are few: exit temperature, quench method, stretch percentage and temper. A supplier who states all four has a process, and one who states none has a habit.

Where Extrusion Sits Among Short Runs

For a small quantity of a custom shape, the press stroke is the shortest part of the calendar. The die and its trial come before it, and the stretch, saw, oven and finish come after it. When a program needs a few hundred meters of a profile before a production tool is justified, low-volume profile extrusion can serve as bridge production between the first samples and that tool.

Sources and Further Reading

Send the Section Drawing of Your Profile

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Profile Extrusion chosen.

Request a Quote