Wall ThicknessInspectionSaw

Aluminum Extrusion Defects and Their Causes in a Production Run

Most rejects in an extrusion run come from the surface and the finishing lines, so agree the visible faces and reject classes before the die is cut.

Short lengths of extruded aluminum profile with visible defects set apart, one with die lines along its face, one with a blister and one with a twisted end, beside good lengths.

Over one year, a Saudi extrusion plant studied by King Fahd University of Petroleum and Minerals returned 322,611 kg (about 356 short tons) of profile from its own press floor to the remelt furnace. That was 1.89 % of 17,069,365 kg extruded. Black and white lines alone accounted for 137,571 kg of it, more than every dimensional fault put together. Off-dimension profile, the defect a buyer’s drawing is written to prevent, came to 959 kg.

Those figures say where a production run loses metal. Most rejects in that plant came from the surface, from handling and from the finishing lines, and comparatively few came from the size of the section. A buyer who knows which defect forms at which step can ask the right questions before the first billet and read a reject report afterward.

Where Aluminum Extrusion Defects Start in a Run

The KFUPM paper by Arif, Sheikh, Qamar, Raza and Al-Fuhaid sorts a rejected profile by its origin. Four sources cover nearly everything a plant throws back:

  • the billet itself, with slag or other inclusions, scale, internal cracks and undissolved oxides;
  • the tooling, meaning billet and die ovens, dies and mandrels, and the stretcher and roll correction equipment;
  • the push through the die, where pressure, container temperature, friction and ram speed are set;
  • the steps after the press, which are sawing, stretching, roll correction, ageing, anodizing and painting.

The same paper notes a practical difficulty. Many extrusion defects carry no single agreed name, and different plants coin different words for the same flaw. A reject report from one supplier may call a fault “black lines” that another supplier logs as “burn marks”. Agreeing on names, or on reference photographs, is the first step in making two suppliers’ reports comparable.

The authors then group defects by mechanism: metal flow, surface, weld, metallurgical, temperature and speed, equipment and tooling, anodizing and painting. Table 1 follows that grouping and pairs each defect with the cause and the remedy the paper gives.

Table 1. Common aluminum extrusion defects, where they form and the remedy given in the KFUPM paper
Defect Where it forms Cause given Remedy given
Pipe or back-end defect rear third of the extrusion billet surface held at the container wall while the core shears past shell extrusion, machined billet, longer discard, matched billet and container temperatures
Funnel rear of the billet peripheral metal shearing near the die discard set by trial, longer at low extrusion ratios
Blisters near the surface, sometimes only after heat treatment trapped lubricant or air no lubricant with a flat die, shell extrusion, a burp cycle after upsetting
Pick-up surface, score lines 3 to 12 mm (0.12 to 0.47 in) long billet inclusions, poor homogenizing, die deflection; temperature sensitive homogenizing, nitrided dies, die cooling
Die lines surface, along the length imperfections at the die land minimum choked land length, polished land
Transverse weld where one billet joins the next oxidized billet ends, contaminated sheared face welds placed on surfaces that are not seen
Speed cracking edges first, then the face local melting at high exit temperature or speed lower temperature and speed, at a loss of output
Bend and twist along the length unequal flow between cavities or uneven billet heating centered cavities, a balancing cavity, the stretcher
Uneven wall cross-section of a hollow mandrel not centered stop the press and realign the mandrel

A defect belongs to a step. Naming the step tells a buyer whom to ask about it and whether it can be corrected or only scrapped.

Back-End Defect, Skin and Coring at the End of Each Billet

The defect the paper calls most common in 6xxx alloys goes by several names: pipe, extrusion defect, fishtailing or back-end defect. Friction holds the outer layer of the billet against the container wall while the core moves forward past it. Toward the end of the push, that oxide-rich skin is drawn inward and appears as an annular separation, a ring in the cross-section, in the rear third of the extrusion.

Four remedies are listed, and each one gives something up.

Extrusion with a shell uses a dummy block 3 to 5 mm (0.12 to 0.20 in) smaller in diameter than the container, so a thin cylinder of skin and impurities stays behind and is pushed out after each billet. Machining the billet removes the dirty as-cast surface before it reaches the press. A long discard simply stops the push before the defect arrives, leaving a larger butt. Matching the container temperature to the billet’s removes the gradient that drives the worst flow pattern.

A finite element study of a porthole die published in Materials in 2018 by Liu and colleagues shows the same mechanism from inside the tool. Sticking friction on the porthole walls slows the metal at the wall, and the authors state that this friction prevents the billet skin from entering the extruded profile. Dead metal zones sit under the port bridges, where velocity is nearly zero.

A related flaw, the funnel defect, forms at the back of the billet. The KFUPM paper advises that the billet is not extruded to the end and that the discard length is found by trial, longer for low extrusion ratios such as thick rod, because the defect starts earlier there.

Skin and coring are kept out of the profile by giving metal away at the end of every billet. A plant that shortens the butt to raise yield is trading against this defect.

Die Lines, Pick-Up and Streaks on the Visible Face

Surface defects decide whether a profile can be anodized as delivered. The Aluminum Association definition quoted in the KFUPM paper describes die lines as longitudinal depressions or protrusions caused by imperfections on the die surface. Even with an optimum land length, the right temperature and highly polished lands, finer and shallower lines remain, which the authors call micro die lines.

Pick-up appears as intermittent score marks of 3 to 12 mm (0.12 to 0.47 in), often ending in a fleck of aluminum debris. A 2007 Master of Engineering thesis at Auckland University of Technology by Robbie Peris extruded AA6060 at 25, 30, 35, 40 and 45 m/min (82 to 148 ft/min), with exit temperatures rising from 542 to 567 °C (1,008 to 1,053 °F). It identified three kinds of pick-up: normal, die line and lump pick-up. Normal pick-up appeared at every speed and exit temperature tested.

The same thesis measured where the alloy starts to melt. Eutectic melting was detected only above 610 °C (1,130 °F) in that material, although 555 °C (1,031 °F) is the lowest melting point for a 6xxx alloy when Mg2Si and excess silicon are present. Exit temperature in the plant was read about 1 m (3.3 ft) from the die and had to be corrected for the drop over that distance.

Streaking shows only after etching and anodizing. A 2012 thesis at the same university by Joshua Walker found etch pits to be the primary cause in the product studied, with grain boundary grooves insignificant. Near the top layer a glossy streak appeared, then dull bands as more metal was removed. The author concludes that the effect is subsurface to a small depth and that abrasive blasting followed by a short etch can resolve it.

The KFUPM paper lists the remaining metallurgical faults on the face:

  1. Streaks from a difference in microstructure between the streaked band and the rest of the surface, which etches and anodizes differently.
  2. Hot spots, dark rough patches from coarse precipitation where adjacent parts of the section cool at different rates.
  3. Spangle, a grainy look from attack that depends on grain orientation.
  4. Silicon marks, black burn marks from very hard particles in the billet.

Of these, hot spots cannot be removed once they form, and the paper’s only remedy is to keep hot profile in contact with the run-out table for the shortest possible time. Streaks from die design or welds also resist mechanical treatment, while a suitable discard normally removes streaks that come from the back-end defect.

Weld Lines From Billet-on-Billet Extrusion

Most plants now extrude billet on billet, holding the back of one billet in a welding chamber or feeder ring so the next can weld to it. Billet ends are always oxidized, and the sheared face picks up stray lubricant and oxide from the shear blade. The joint, called a transverse weld, is therefore usually a discontinuity in the profile.

In a solid section the transverse weld runs out to the surface. Through a hollow it also meets the longitudinal weld lines formed where metal split by the port bridges joins again in the welding chamber. The KFUPM remedy is a design one: place the welds on faces that are not seen in the finished product.

Black lines belong to the same zone; logged together with white lines, they formed the largest single reject class in the plant data. The paper attributes them to local high pressure in the welding chamber of a hollow die, or to any aberration in a solid die, and notes they generally become visible only after etching. A profile can pass inspection at the press and fail at the anodizing line for a cause that was set in the die.

Weld position is fixed when the die is designed. A drawing that marks the visible faces gives the die maker the information needed to keep welds off them.

Exit Speed, Temperature and the Cracking Limit

Heat generated at the die rises quickly with exit speed, because more work goes in and less heat escapes to the tooling. At a high enough speed the surface melts locally. The KFUPM paper describes the resulting hot shortness, tearing that starts at the edges and spreads across the face as fir-tree or speed cracking.

The porthole die study gives numbers for one case. Its authors cite a temperature rise of more than 100 °C (180 °F) from billet to extruded profile and set 560 °C (1,040 °F) as the critical temperature for AA6063, above which hot tears and low mechanical properties follow. Their optimized die reached a maximum of 539.3 °C (1,003 °F), starting from a 480 °C (896 °F) billet.

Lower temperature and speed avoid these defects, and the paper is plain about the trade: output slows. The working window sits between the speed that tears the surface and the speed the schedule wants, and its width depends on the alloy, the die and the section.

Bend, Twist and Uneven Wall From Unequal Metal Flow

Shape defects come from metal leaving the die at different speeds across the section. The Liu study measured this on a profile 107.57 mm (4.235 in) long with a minimum wall of 2.525 mm (0.099 in), a cavity only 4.04 mm (0.159 in) across and a length to width ratio of 42.6. With the first die design, metal at the solid end left at 182.3 mm/s (7.18 in/s) while metal near the cavity left at 111.0 mm/s (4.37 in/s), against a theoretical 151.8 mm/s (5.98 in/s). The faster region pushed on the slower one and the profile bent along its length.

The authors corrected the die in three steps: they moved the welding chamber into the upper die and opened the porthole entrance angle to 30°, added baffle plates to feed more metal to the cavity side, and finally changed bearing lengths, longer where metal ran fast and shorter where it ran slow. Table 2 shows what each measure did.

Table 2. Porthole die study results before and after correction, AA6063, 210 mm (8.3 in) container, ram 2 mm/s (0.08 in/s), Liu et al. 2018
Measure Initial die Corrected die
Standard deviation of exit velocity 19.63 mm/s (0.773 in/s) 0.448 mm/s (0.018 in/s)
Velocity spread across the section, final step 7.71 mm/s (0.304 in/s) before bearing change 2 mm/s (0.079 in/s)
Largest upper die displacement 0.107 mm (0.0042 in) 0.05945 mm (0.0023 in)
Mandrel tip displacement 0.0925 mm (0.0036 in) 0.04648 mm (0.0018 in)
Extrusion load 10,617.3 kN (about 1,193 US tons-force) 13,903.2 kN (about 1,563 US tons-force)

The corrected die raised the load, which the paper links to die wear, yet stayed within the 2,000 ton press used for the trial. In the plant trial, after stretching and straightening, no distinct bend or twist was found, and the wall at the small cavity differed from the required size by 0.1 mm (0.004 in).

The KFUPM paper gives the plant-floor version of the same problem.

In a multi-hole die, unequal flow between cavities bends or twists the strands, and an unevenly heated billet does the same. Cavities are centered for equal flow, and an extra cavity is sometimes added for symmetry. Minor bends are corrected on the stretcher and an out-of-angle section on the roll correction machine. An uneven wall in a hollow means the mandrel is off center, and the remedy given is to stop the press and realign it.

Handling, Anodizing and Painting Rejects After the Press

The press is not the only reject station.

In the KFUPM data, scratches and damage at the press came to 86,075 kg, a quarter of press rejects. Runout or graphite marks form where heavy hot sections rub on graphite conveyor rolls, and die stop marks form whenever the press pauses. Saw oil that splashes onto hot profile burns into stains, which the paper suggests avoiding by placing the saw far enough from the press for the metal to cool. In multicavity dies, strands rubbing together leave hot rub marks, prevented by graphite separators.

Anodizing adds its own faults.

Black pits form when rinse water is contaminated and profiles stay immersed too long. Too long in the caustic etch removes more surface than intended and leaves a dull, grainy finish. A profile that is etched and anodized again after a failed first pass loses more wall, and the paper records such pieces being scrapped for reduced wall thickness. Painting lines reject for thin film, dust and orange peel, blisters that survived from the press, and profiles that touched and stuck together in the oven.

Table 3. One year of rejects by station in the plant studied, from the KFUPM paper’s Table 1
Station Output Rejected Reject rate Largest classes
Press 17,069 t (18,816 short tons) 323 t (356 short tons) 1.89 % black and white lines 42.6 %, scratches and damage 26.7 %
Anodizing 10,052 t (11,080 short tons) 150 t (165 short tons) 1.49 % black pits 27.7 %, damage 27.6 %, process scrap 24.8 %
Painting 1,532 t (1,689 short tons) 95 t (105 short tons) 6.20 % other 41.5 %, thin film 35.5 %, dust and orange peel 21.4 %

Dimensional faults made up a small part of the press figure. Concave or convex faces, twist and bends, out-of-angle and off-dimension sections together came to 22,652 kg, about 7.0 % of press rejects. Low hardness from ageing furnace faults added 11,196 kg.

In this plant the largest rejects were cosmetic and the highest rate was at the paint line. A buyer of painted profile has more reason to inspect the finish than the section.

Reading Reject Data for a Production Run

The paper’s model treats each station as a probability of producing a defective piece. A profile rejected at painting has already been through billet preparation, the press, ageing and pretreatment, so a reject late in the chain carries all the work done before it. That is why a paint-line rate of 6.20 % weighs more than its share of tonnage suggests, and why the authors group rejects by press, anodizing and painting rather than by mechanism when they count them.

For a buyer planning a run, the defect list turns into a short set of agreements before the die is cut:

  • which faces are visible, so welds and die lines can be kept off them;
  • whether the profile will be anodized, painted or left mill finish, because streaks and black lines may show only after etching;
  • the sample length and positions taken from each run, including pieces from near the back of a billet where coring appears;
  • which defects may be corrected on the stretcher or roll correction machine and which mean scrap;
  • names or reference photographs for each defect class, so reports from two suppliers mean the same thing.

The first lengths from a new die are where most of these questions are answered. Flow balance, weld position and surface quality are fixed by the die, and the Liu study shows that correcting them can take several design passes. When a program needs a few hundred lengths to prove a section before it commits to volume, low-volume profile extrusion and bridge production are where to agree the visible faces, the sample positions and the reject classes before the first billet is pushed.

Sources and Further Reading

Send the Section Drawing of Your Profile

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Profile Extrusion chosen.