Meaning
Skin and coring are the billet defects that the butt allowance keeps out of an aluminum profile, the skin being its oxide-rich surface. Their presence explains why every push ends with metal thrown back. Where they reach the profile, they show as defects near the back end of a push.The Butt Allowance
Light Metal Age sets the usual allowance at 12 to 14 % of the billet’s weight. That share stays in the container as the butt, carrying the skin with it. Sheared away during the next billet’s loading, the butt goes back for remelting. A University of Illinois thesis gives the butt as about 10 % of billet length.Read More
The Trade-Off
The butt length is a compromise either way. Stopping the push at 14 % leaves a long butt that is hard to shear cleanly. A butt pushed down to 25 to 50 mm (1 to 2 in) has the opposite fault. Contamination then collects in the die and at the tail of the bar. Longer billets also leave longer butts.Container Temperature
Temperature at the liner affects how much skin flows into the profile. Flow near the liner wall differs from flow along the billet’s axis. Light Metal Age reports modeling of a container held at least 28 °C (50 °F) below the billet. Less skin flowed into the profile. It also gave better productivity.Where It Shows
Skin or oxide that does get through shows as streaks or blisters toward the tail of the push. Samples from the end of a length test that worst case. A buyer asks which part of the push a sample came from.