Anodized Film Thickness and Color Tolerance on Extruded Profiles

Specify anodic film as an ISO 7599 class on marked faces, and agree color against limit samples before the first lot is anodized.

Short lengths of the same extruded aluminum profile anodized in close shades of bronze and in natural silver.

A reading taken 4 mm from a rack contact mark does not count. ISO 7599:2018, the standard for specifying decorative and protective anodic coatings, says thickness is measured on the significant surfaces and never within 5 mm (0.2 in) of the areas of anodic contact or close to a sharp edge. That one clause explains much of how anodized thickness is toleranced: the number belongs to the faces a buyer sees, measured in a defined way, and judged against a minimum rather than a plus-or-minus band.

Color is handled differently again. No document opened for this article prints a single color tolerance figure for anodized aluminum. The same standard asks the customer to state the color and the maximum limits of color variation, preferably by agreed limit samples. A buyer who writes “clear anodize” or “black anodize” and nothing else has specified neither a thickness nor a color.

How Anodized Film Thickness Is Specified and Accepted

ISO 7599:2018, published in Europe as EN ISO 7599:2018 and in Britain as BS EN ISO 7599:2018, lays down the method. Its contents run from the information the customer supplies to the anodizer, through coating thickness, sealing, appearance and color, to a normative annex on interpreting average and local thickness. The 2018 edition replaced the 2010 one, which BSI lists as withdrawn on 23 February 2018, and changed the title from “General specifications” to “Method for specifying”. It does not cover hard anodizing, which ISO 10074 treats.

The standard leaves the key choices to the order. Clause 4.2 lists what the customer supplies in every case, among them a reference to ISO 7599, the intended service use, the significant surfaces, the surface preparation, the thickness class, whether the finish is clear or colored, and whether and how it is sealed. It states that the required thickness “shall always be specified”.

Qualanod, the quality label for sulfuric acid anodizing, builds certification on top. Its technical note on weathering states that the Qualanod specifications require the anodizer to meet requirements on coating thickness, sealing, light fastness and surface abrasion resistance, and require the contract between customer and anodizer to specify the alloy, the coating thickness class, the appearance, and the cleaning and maintenance procedures. Qualanod’s architectural applications page lists the product criteria an inspection checks: visible defects, surface texture and color, coating thickness, coating quality, sealing quality and light fastness.

In North America, the Aluminum Anodizers Council points specifiers to AAMA 611 for architectural anodizing and to the Aluminum Association designation system for naming the finish. Military and aerospace work refers to MIL-A-8625, which the council describes as covering six types and two classes, and which expects the coating thickness to be called out on the purchase documents or the drawing.

Thickness is specified as a class, and the class is a minimum average with a minimum local value beside it. The drawing names the class and the faces it applies to.

Thickness Classes in Microns and Mils

The Aluminum Association system, as reproduced by the Aluminum Anodizers Council, names an anodic finish with the letter A and two digits. Its first digit groups the thickness and the second names the color method: clear, integral color, impregnated color or electrolytically deposited color.

Table 1. Anodic coating thickness designations and recommendations, from the Aluminum Anodizers Council and Hydro
Designation or use Thickness Source
A21 to A24, protective and decorative less than 10.2 µm (0.4 mil), value to be specified Aluminum Association system via AAC
A31 to A34, Architectural Class II 10.2 to 17.8 µm (0.4 to 0.7 mil) Aluminum Association system via AAC
A41 to A44, Architectural Class I 17.8 µm (0.7 mil) and thicker Aluminum Association system via AAC
Normal stress indoors 10 µm (0.39 mil) Hydro recommendation
Chemical contact indoors 15 µm (0.59 mil) Hydro recommendation
Normal to high stress outdoors 20 µm (0.79 mil) Hydro recommendation
Corrosive or abrasive exposure 25 µm (0.98 mil) Hydro recommendation
Color anodizing minimum 20 µm (0.79 mil) Hydro recommendation

The council’s example of a full interior panel callout is AA-M42C21A34: a fine matte nondirectional mechanical finish, a fine matte chemical etch, and an Architectural Class II coating with electrolytically deposited color. Its note adds that the finisher and customer decide, by sampling or discussion, exactly which process makes the M42 and C21 parts. The designation fixes the thickness band; it leaves the look to an agreed sample.

The same council warns about the thin end. Anodized sheet at the bottom of the market is often sold with a coating of 0.15 mil, about 3.8 µm, which it describes as unlikely to last more than a few years in exterior architectural use and even less on the coast. Dyed finishes suffer most, because a thinner coating holds less dye and fades sooner.

Hydro’s anodizing brochure for extruded profiles states that sulfuric acid anodizing at room temperature runs until the desired film thickness is reached, generally up to 25 µm (0.98 mil). For hard coatings the reference changes. The council’s MIL-A-8625 page gives “Type III, Class 2 black, 2.0 mil coating thickness” as an example, a dyed hard coat of about 51 µm.

Average Thickness, Local Thickness and the 80 Percent Rule

ISO 7599 grades anodic coatings by their minimum average thickness in micrometers, written as AA followed by the grade. Each typical class also carries a minimum local thickness, the lowest value any single measuring area may read.

Table 2. Typical coating thickness classes, ISO 7599:2018, Table 1
Class Minimum average thickness Minimum local thickness
AA 5 5.0 µm (0.20 mil) 4 µm (0.16 mil)
AA 10 10.0 µm (0.39 mil) 8 µm (0.31 mil)
AA 15 15.0 µm (0.59 mil) 12 µm (0.47 mil)
AA 20 20.0 µm (0.79 mil) 16 µm (0.63 mil)
AA 25 25.0 µm (0.98 mil) 20 µm (0.79 mil)

The local column is always 80 % of the average. ISO 7599 allows higher or intermediate averages where particular surface properties are wanted, but in no case may the minimum local thickness fall below 80 % of the minimum average. How average and local readings are interpreted on a test specimen is set out in its normative Annex C.

A worked case shows the scale. Under AA 20, a single reading of 15 µm fails the local floor of 16 µm even if the piece averages 21 µm. A profile with one thin face can pass on average and still fail.

Two further provisions shape the choice. Where corrosion resistance is paramount, anodizer and customer may agree a minimum local thickness with no restriction on the average. And some dyestuffs need class AA 20 or higher to absorb enough dye and hold their light fastness, which matches Hydro’s 20 µm minimum for color anodizing.

Both values apply only on the significant surfaces. ISO 7599 says these are indicated preferably by drawings or by marked test specimens, and that different parts of a significant surface can carry different requirements. On a profile with hidden channels and back faces, the drawing that marks the significant surfaces also decides where a thinner film is acceptable.

The class minimum governs the average and the 80 % floor governs every single reading.

Why the Class Decides Service Life

ISO 7599 states the reason for the class plainly: protection against pitting corrosion of the aluminum increases with coating thickness, so product life depends heavily on it. Qualanod’s technical note on weathering, edition of 3 August 2011, explains the mechanism. Aggressive chemicals have to dissolve or penetrate the anodic coating before a pit can start, and the protection depends primarily on coating thickness and is largely independent of sealing quality. Good quality anodized aluminum loses thickness slowly in service, and pitting begins once enough has gone.

The note collects outdoor exposure data on how fast that loss runs. Its summary gives about 0.2 to 0.4 µm per year in urban air, similar or lower in marine air, about 0.05 µm per year at best for 25 to 30 µm coatings, and 1.2 µm per year at worst in the polluted Sheffield of the 1970s. It also finds that the rate falls over time and that a thicker coating never ends thinner than a thinner one exposed for the same period.

Table 3. Thickness loss of anodic coatings exposed 1964 to 1980, from Qualanod’s weathering note (data of B.R. Ellard)
Site Initial thickness Loss rate Final thickness
Banbury, rural 25 µm (0.98 mil) 0.05 µm (0.002 mil) per year 24 µm (0.94 mil)
Leeds, urban 25 µm (0.98 mil) 0.3 µm (0.012 mil) per year 20 µm (0.79 mil)
Manchester, urban 25 µm (0.98 mil) 0.35 µm (0.014 mil) per year 19.5 µm (0.77 mil)
Portsmouth, marine 30 µm (1.18 mil) 0.15 µm (0.006 mil) per year 27.5 µm (1.08 mil)
Sheffield, industrial 15 µm (0.59 mil) 0.55 µm (0.022 mil) per year 6.5 µm (0.26 mil)
Sheffield, industrial 25 µm (0.98 mil) 0.65 µm (0.026 mil) per year 14.5 µm (0.57 mil)

The note adds that ISO 7599:2010 classifies thicknesses and gives guidance on choosing them, but that the advice is general, because micro-climate, orientation on the building and prevailing wind change the outcome. Those figures show why the margin matters: the 15 µm coating in Sheffield ended at less than half its starting thickness.

Measuring Anodic Film by Eddy Current and Micro-Section

ISO 7599:2018 names three methods and their order of authority:

  1. Cross-section examined by microscope to ISO 1463 or ISO 9220, the referee method in a dispute.
  2. Eddy current to ISO 2360, with the instrument calibrated to the maker’s instructions using calibration standards before any measuring; Annex D describes those standards, and BSI lists its revision among the changes from 2010.
  3. The split-beam microscope of ISO 2128.

Readings are taken on the significant surfaces as Annex C directs, away from sharp edges and at least 5 mm (0.2 in) from contact areas, and both the local readings and the average per piece are recorded so that both limits can be applied. The Aluminum Anodizers Council lists the methods a North American specification may call: ASTM B244 for thickness by eddy current, ASTM B137 for coating mass, ASTM B680 for seal quality, and ISO 2360 and ISO 3210.

Thickness is also a dimension. Hydro’s brochure diagram of converted layer behavior shows the oxide sitting partly above the original metal surface and partly below it, marked one third and two thirds, and the Aluminum Anodizers Council states that the coating is about 30 % thicker than the metal it replaces. Either way, part of the film builds outward on every coated face while part consumes metal beneath it, which matters on slots and fits held to a few hundredths of a millimeter.

Heat sets a separate limit. Hydro states that fine cracking can appear in the oxide above 100 °C (212 °F) and is more noticeable the thicker the layer, and that thicker layers reduce gloss. A specification that asks for more thickness than the use needs can make the finish look worse in a hot location.

Sealing, Abrasion and Sampling Checks

Thickness is rarely the only test. ISO 7599 describes sealing as a treatment that reduces the porosity and absorption of the coating. Where the initial appearance is to be retained outdoors, sealing at the surface matters; where the part meets strong acids or alkalis for short periods, such as car-wash fluids, sealing through the whole thickness can matter. Hydrothermal sealing is called very well established, and its test methods can be applied to other sealing treatments.

In a dispute, hydrothermal sealing quality is judged by one of the mass loss methods of ISO 3210. Whether a prior acid treatment is used and the maximum accepted loss of mass are agreed between anodizer and customer; the standard recommends the acid step for external architectural coatings and not for internal or decorative ones, and notes that the maximum is variously set at 30 or 40 mg/dm2 (0.3 or 0.4 g/m2). These methods test the surface, not the whole thickness of the coating.

Abrasion is checked on thicker architectural films. Qualanod’s technical note of 24 March 2025 states that it currently assesses surface abrasion resistance on architectural coatings with an average thickness of 20 µm (0.79 mil) or more, by two methods:

  • a manual glass paper method based on method 1 of ISO 18771, used for production control;
  • an abrasive wheel wear test based on ISO 8251, used as the referee test.

Because consistent glass paper became hard to source, Qualanod is introducing chemically etched glass files of standardized float glass as an equivalent production control tool. The original method, the note explains, was devised to detect soft films that can later chalk in service.

Sampling itself is left to the order. ISO 7599 says sampling procedures are specified by the customer, with ISO 2859-1 as guidance, and that test specimens are production components wherever practicable. Where special specimens are agreed, they are of the same alloy and go through the anodizing line at the same time as the parts.

Color Tolerance on Anodized Extrusions

The Aluminum Anodizers Council is direct about color. Anodized coatings show excellent color consistency, it says, but anodizing does not give perfectly consistent color, and buyers are advised to have metal for one job processed at the same time and in the same place wherever possible. The council discourages the word “range” for color, because lightness is only one of several dimensions of appearance, and recommends measuring color, lightness and gloss against an approved standard.

Its suggested specification text says that an acceptable range is agreed between the specifier-buyer and the manufacturer-anodizer on a per-project basis. Appearance, it notes, depends on more than depth of color: alloy, temper, gloss, surface structure and the coloring process all move it. Hydro adds profile shape, the lighting and angle of view, and the thickness of the layer, and calls anodized aluminum a living material for that reason.

Alloy enters directly. The council’s alloy table notes that silicon in 6063 can give the coating a gray or brown tint, and that chromium in 6061 gives thicker coatings a yellowish tint. Two extrusions anodized side by side in the same tank can therefore differ in shade because they were pressed from different alloys.

The press shows through as well. Guidance from the council on mechanical finishing notes that uncolored anodic oxide is transparent or translucent and follows the surface texture, so surface defects such as die lines are not covered up by anodizing; they are removed mechanically before the line or accepted on the limit samples.

Color also moves in service. Qualanod’s weathering note says that many dyestuffs can change color within a few years outdoors, that certain dyestuffs resist fading and suit architectural use when applied correctly, and that electrolytic coloring produces lightfast deposits. Hydro’s electrolytic color scale runs from C-0 natural through C-31 champagne and C-32 to C-34 bronzes to C-35 black.

In practice, the agreed limit samples become the approved sample against which every later lot is judged.

Color tolerance is a pair of agreed limit samples and an agreed way of viewing them. Without them, two lots can both be “black anodized” and still not match.

What the Drawing and Order Should Say

ISO 7599 lists the information the customer supplies, and the items that decide thickness and color can be written straight onto the drawing or order:

  • the standard and edition, such as ISO 7599:2018, AAMA 611 or MIL-A-8625, and the thickness class;
  • the significant surfaces, marked on the drawing, and the preferred position and maximum size of contact marks;
  • clear or colored finish, the coloring process, the color and its limit samples;
  • whether and how the coating is sealed, and any sealing, corrosion or abrasion requirements;
  • the sampling plan, and the alloy held the same across lots where color matters.

First lots are where these choices are tested on real profiles. When a profile needs its first anodized lengths approved for thickness and color before volume, low-volume profile extrusion and bridge production are where the class, the significant surfaces and the limit samples are fixed before the first lot is racked.

Sources and Further Reading

Send the Section Drawing of Your Profile

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Profile Extrusion chosen.

Request a Quote