Meaning
A temper is the code after an aluminum alloy number, such as T5, T6 or O, that states how the metal was treated. It is written with the alloy, as in 6063-T5, and governs the strength the certificate guarantees. North American designations follow ANSI H35.1, and European ones follow EN 515. Two profiles of one alloy in different tempers can differ by a factor of three in guaranteed yield.Letter Definitions
Hydro’s datasheets restate the EN 515 definitions. A T4 profile is solution heat treated, then left to age at room temperature. In T5 it cools from the hot shaping step and goes straight to an aging oven. In T6 it is solution heat treated before that oven. T64 stops aging early for better forming, and T66 lifts T6 through special process control. O is the annealed state.Read More
Where It Is Set
For 6000-series profiles the first step of a T5 or T6 happens in the press. The metal leaves the die hot enough to count as solution treated, and the quench fixes that state. Aging then runs in separate ovens, and the time and temperature trade against each other. Hydro marks several 6063 tempers, T6 among them, as obtainable by press quenching. A temper letter on the order is therefore a statement about the press line as well as the oven. Exit temperature, quench method, stretch and temper together describe a repeatable procedure.Strength by Temper
The temper moves the guaranteed figures more than any other line on the order. For EN AW-6063 up to 10 mm (0.39 in), yield rises from 65 MPa (9.4 ksi) in T4 to 130 MPa (18.9 ksi) in T5. T6 adds 40 MPa, to 170 MPa (24.7 ksi), and T66 reaches 200 MPa (29.0 ksi). At the 10 mm boundary T5 loses 20 MPa of guarantee, while T6 loses only 10 MPa. On EN AW-6082, the guaranteed yield climbs about 2.4 times between T4 and T6. A weld changes the temper locally, so the table figures do not hold at a welded joint.Tempers by Table
Each table lists only the tempers it covers for an alloy. Hydro’s 6005A sheet prints T4 and T6, with no T5 row. The Aluminum Association’s table gives the same alloy T1, T5 and T61 instead. A temper asked for on an order is checked against the table that will certify it.Hardness Check
Hardness tracks the temper and is easy to read on a sample bar. For 6063, Hydro lists typical readings of 50 HBW in T4, 65 HBW in T5 and 75 HBW in T6. Those readings are given for information, and the table guarantees none of them. A low reading after aging still points back to the quench or to the oven time and temperature.Bounded Tempers
Most limit rows are minimums, and a few tempers carry a ceiling as well. Annealed 6061-O sets maximums of 152 MPa (22.0 ksi) tensile and 110 MPa (16.0 ksi) yield. The producer temper 6063-T52 asks for 152 to 207 MPa (22.0 to 30.0 ksi) tensile. A tensile result above such a ceiling rejects the lot, though a T6 lot would accept the same figure.Tolerance Effects
The temper also changes the dimensional tables. ANSI H35.2 gives the O temper its own straightness rows and four times the standard flatness. For the stress-relieved TX510 group, T6510 among them, the form values are left to agreement between purchaser and vendor. The TX511 group has printed rows. The AEC manual advises a stress-relieved temper such as TX511 for parts that will be machined or cut from asymmetrical shapes.Order Line
The temper is written in full on the drawing and the order, in ANSI H35.1 form. Writing 6082-T6511 asks for a stress-relieved profile, which plain T6 does not satisfy. Under the footnotes to the Aluminum Association’s table, a user can usually reach T6 properties by solution heat treating from O or F. A part formed or worked in between may come out lower, so the certificate speaks for the product as shipped.