A sulfuric acid anodizing tank, as the Aluminum Anodizers Council describes the common process, holds a 15 % acid solution at about 21 °C (70 °F) and drives about 1.3 A/dm2 (12 A/ft2) through the work at 18 to 24 V for 10 to 60 minutes. Out of that comes a film of 2.5 to 25 µm (0.1 to 1.0 mil). Every number in that sentence is a lever, and the profiles on the rack respond to each of them.
Anodizing is often drawn as one box on a process chart. It is in fact a line of tanks, each with its own chemistry and its own way of spoiling a profile, and the appearance of the finished extrusion is set as much by the steps before the anodizing tank as by the tank itself.
The Anodizing Line From Rack to Seal
Hydro’s anodizing brochure for extruded profiles lays out the line in the order the profiles travel. The Aluminum Anodizers Council groups the same work into five stages: cleaning, pretreatment, anodizing, coloring and sealing. Put together, the sequence for an extrusion runs as follows:
- Racking, where each profile is fixed with an electrical contact.
- Degreasing, which removes oil and dirt.
- Etching in caustic soda, or chemical brightening for a specular finish.
- Rinsing, then desmutting in an acid bath to remove the film of alloying elements left by the etch.
- Anodizing, with the profile as the anode in dilute sulfuric acid.
- Rinsing, twice in Hydro’s chart.
- Coloring, if a color other than natural is wanted.
- Sealing, which closes the pores of the oxide.
Rinsing runs between the process baths. Hydro notes that it works in cascades, so that chemicals are not carried from one bath into the next and each bath stays stable. A mechanical finish, if one is specified, comes before all of this.
The anodizing tank is step five of eight. A profile can be spoiled in any of the four steps before it and in the three after it.
Racking the Profiles and Making Contact
Anodizing is an electrochemical process, and Hydro states plainly that parts are fixed with an electrical contact. The council calls the method used for extrusions batch anodizing: parts are racked and immersed in a series of tanks, which separates it from coil anodizing, where sheet unwinds continuously through the line.
The contact point leaves a mark. ISO 7599:2018, the standard for specifying decorative and protective anodic coatings, acknowledges this when it rules out thickness readings within 5 mm (0.2 in) of the areas of anodic contact, and it lists the preferred position and maximum size of contact marks among the information a customer may give the anodizer. A buyer who marks the significant surfaces on the drawing also tells the anodizer where the contacts can go.
Rack position matters for handling as well. The KFUPM study of a Saudi extrusion plant counts profiles that fell into tanks because of bad clamping among its anodizing rejects: 3,438 kg in one year, in a line that anodized 10,051,677 kg and rejected 149,770 kg, or 1.49 %.
Mechanical Finishing Before the Line
Texture applied by hand or machine goes on first. The council lists buffing, polishing, sanding, sand blasting and shot peening as mechanical finishes, done before chemical finishing or anodizing.
What the council says next is the point for an extrusion buyer. Uncolored anodic oxide is transparent or translucent and follows the surface texture, so surface defects and applied textures both show through. Anodizing does not hide die lines, scratches or handling marks. They are removed mechanically before the line or accepted.
The Aluminum Association system, as the council reproduces it, gives these finishes M codes, from M11 for specular as fabricated to M45 to M47 for fine, medium and coarse shot blast. A study of streaking on extrusions at Auckland University of Technology found that abrasive blasting followed by a short etch resolved the streaks it examined, which shows the mechanical and chemical steps working together.
Cleaning, Etching and Brightening
The council’s typical chemical treatment has three parts: an inhibited acid or alkaline cleaner to remove dirt and oil, a deoxidizing dip in strong acid to remove natural oxide or heat-treat scale, and then a chemical etch or a brightening step. Cleanliness, it says, decides anodizing quality.
Etching sets the matte look of most anodized extrusions. A weak caustic soda solution removes metal evenly and roughens the surface to a uniform matte. The council’s designation tables give one recipe for the medium matte finish C-22: sodium hydroxide at about 30 to 45 g/L (4 to 6 oz/gal) at 60 °C (140 °F) for 5 minutes. Acid etching with ammonium bifluoride or trisodium phosphate gives a white satin finish while removing less metal.
Brightening goes the other way. A concentrated mix of phosphoric and nitric acids, or an electrochemical bath, levels the surface by removing the micro-peaks while leaving the micro-valleys, which is how a near-mirror finish is reached. The AA designation is C31. Hydro adds that alloy 6463 gives a brighter finish and that the shade and matteness of an etched surface depend largely on the alloy chosen.
The etch is also where a profile loses metal it cannot get back. Three faults from this stage appear in the KFUPM paper:
- too long in the caustic tank removes more surface than intended and leaves a grainy, dull finish;
- a profile left too long before rinsing keeps caustic on the surface, which does not rinse off and leaves caustic patches;
- a lot that fails and is etched and anodized again loses more wall each time, and the plant studied scrapped 8,286 kg in one year for reduced wall thickness.
The council recommends choosing the exact etch from sample coupons of several versions of the finish, picking the one closest to the look wanted. For an extrusion program, the coupon is the profile itself, etched on the line it will run on.
Etch time takes metal off every face. A profile with a thin wall or a tight fit has less to give, and a second pass through the line takes more.
Inside the Anodizing Tank
In the anodizing bath the profile is connected as the anode, which gives the process its name, and Hydro places the cathodes around the sides of the tank. The aluminum surface is converted electrochemically into oxide, and the process continues until the desired film thickness is reached, generally up to 25 µm (0.98 mil) in Hydro’s practice.
| Process | Electrolyte | Temperature | Current density | Voltage | Time | Film |
|---|---|---|---|---|---|---|
| Sulfuric acid | 15 % solution | 21 °C (70 °F) | 1.29 A/dm2 (12 A/ft2) | 18 to 24 V | 10 to 60 min | 2.5 to 25 µm (0.1 to 1.0 mil) |
| Organic acid, integral color | 90 to 100 g/L (12.0 to 13.4 oz/gal) organic acids with a little sulfuric | 21 to 27 °C (70 to 80 °F) | 2.58 A/dm2 (24 A/ft2) | up to 75 V | not stated | amber, bronze and black films |
| Hard anodizing | special electrolytes | very low | high | not stated | not stated | usually over 25 µm (1.0 mil) |
The oxide grows from the metal rather than sitting on top of it. According to the council, the coating is about 30 % thicker than the metal it replaces, because the oxide takes more volume than the aluminum consumed. Hydro’s brochure diagram shows the converted layer sitting one third above the original surface and two thirds below it. Either way, a profile leaves the tank slightly larger on every coated face than it went in.
Hard anodizing is a separate regime. The council describes films usually thicker than 25 µm, made at very low temperature and high current density for wear surfaces such as pistons and cylinders. Hydro notes that sealing improves the corrosion resistance of a hard anodized surface but reduces its hardness, and the council adds that hard coats are often left unsealed.
Process control is the anodizer’s side of the job. The council describes power and color application as preprogrammed and verified on each batch, with statistical process control used by many plants to hold film thickness, density, color uniformity and sealing to the specification.
Coloring the Open Pores
After anodizing, the oxide is porous, and color goes into the pores before they are sealed. Hydro describes two families: dyes taken up by unsealed natural anodized aluminum by dipping or spraying, and electrolytic coloring, a separate stage where a tin salt is deposited at the bottom of the pores by alternating current, giving shades from champagne to black. The council lists tin, cobalt, nickel and copper as the metals commonly used.
| Method | How the color forms | Minimum film | Shades |
|---|---|---|---|
| Integral coloring | one step, special alloy and organic acid | film 15 to 40 µm (0.6 to 1.6 mil) | brown, bronze, gray, slate; no white |
| Organic dyeing | dye absorbed without current | 20 µm (0.79 mil) | spectral colors; no brown, bronze or gray |
| Inorganic dyeing | metal oxide hydrates in the outer coating | 20 µm (0.79 mil) | pale to dark bronze and gold |
| Electrolytic coloring | metal deposited at the base of the pores by current | 20 µm (0.79 mil) | brown, bronze, gray, slate, black, pink, burgundy; no white |
| Electrolytic plus organic | one color at the pore base, one in the coating | 20 µm (0.79 mil) | muted shades, no white |
Hydro’s brochure gives the same 20 µm minimum for color anodizing in general. Interference coloring is a newer method: the council describes sulfuric anodizing, an electrochemical change to the pore shape, and tin deposition, giving lightfast blues, greens and other colors. It also warns that color variation in these finishes tends to show as a change of hue rather than of lightness, and that anodizer and customer should define the accepted color in advance.
Integral coloring, the council notes, needs significantly more electrical power than the other methods. Hydro adds a caution on light fastness: some inorganic colors have limited fastness and do not suit high temperature or strong UV exposure.
Sealing and the Checks That Follow
Sealing closes the pores. The council describes the result as a surface that resists staining, abrasion, crazing and loss of color. Hydro’s standard practice is immersion in water close to boiling, with alternative processes at lower temperatures. ISO 7599 calls hydrothermal sealing very well established, with its own quality control methods, and BSI notes that the 2018 edition admits sealing methods beyond hydrothermal and cold nickel fluoride sealing.
Sealing quality is checked after the fact. In a dispute, ISO 7599 judges hydrothermal sealing by the mass loss methods of ISO 3210, with any prior acid treatment and the maximum loss agreed between anodizer and customer; it recommends the acid step for external architectural coatings and notes that the maximum is variously set at 30 or 40 mg/dm2 (0.3 or 0.4 g/m2). The same standard lists eddy current to ISO 2360 among its thickness methods, with a microscope cross-section as the referee if results are disputed.
The seal is the last wet step and the one that cannot be seen. It is proven by a test on a sample, not by looking at the rack.
What Goes Wrong on the Line and How It Shows
Most anodizing faults appear as a change in appearance rather than in size, and several trace back to the extrusion press. The KFUPM paper explains that streaks, hot spots and spangle on anodized extrusions come from differences in microstructure that respond differently to etching and anodizing.
| Fault | Step | How it shows | Source |
|---|---|---|---|
| Black pits | rinsing | small local corrosion spots; 41,540 kg in one plant-year | KFUPM paper |
| Dull, grainy finish | etching too long | loss of the intended matte | KFUPM paper |
| Caustic patches | delayed rinse after etch | patches that do not rinse off | KFUPM paper |
| Reduced wall | repeated etch and anodize | wall below drawing; scrapped | KFUPM paper |
| Streaks | etch on varying microstructure | lighter or darker, glossier or duller bands | KFUPM paper; AUT thesis |
| Fallen in tank | racking | sections dropped by bad clamping; 3,438 kg in one plant-year | KFUPM paper |
| Bloom, chalking, staining | sealing and anodizing quality | can appear in the first year outdoors on poor quality product | Qualanod weathering note |
| Fine cracking | service | crazing above 100 °C (212 °F), worse on thick films | Hydro brochure |
Alloy choice belongs on the same list, because it decides the color the oxide takes before any dye is added. The council’s alloy table rates 6063 and 6463 among the anodizing quality extrusion alloys and lists 6061 and 6101 as not of anodizing quality, and it notes that 2xxx alloys give a yellow coating with poor protection while 4xxx alloys give dark gray.
Handling Anodized Profiles After the Line
The finished film changes how a profile is handled, joined and cleaned. Hydro describes the oxide as electrically insulating and gives a breakdown voltage of 500 to 600 V for a sealed 15 µm (0.59 mil) layer. An assembly that relies on metal-to-metal contact for grounding or electrical continuity therefore needs a bare area, either masked on the line or machined after it.
Corrosion resistance is good where the pH stays between 4 and 9, in Hydro’s account, while strongly alkaline materials stain and damage the surface. Lime, cement and gypsum on a building site are the examples given, and Hydro recommends protecting visible surfaces with tape until the work around them is finished. For cleaning, it suggests water with a neutral detergent or white spirit and warns against strong alkaline cleaners.
The Aluminum Anodizers Council makes a related point about service life. It describes anodizing as a renewable finish: dirt and stains that build up over years can be removed with a mild detergent and an abrasive cleaning technique, which takes off a small amount of the coating and leaves a renewed surface. The thickness specified at the anodizing line is what that cleaning draws on later.
Gloss also follows thickness. Hydro notes that thicker oxide layers reduce gloss and that the appearance of any anodized surface, natural or colored, changes with the viewing angle because the oxide is transparent. A sample approved flat on a desk can look different on an installed profile seen from below.
Planning Fabrication Around Anodizing
The order of fabrication steps follows from the coating. Hydro’s guidance is that forming takes place before anodizing, because the oxide forms poorly when cold. Welding comes before anodizing too, and the weld filler affects the appearance. Cutting and drilling can be done after anodizing, but the new surfaces are bare.
Two more decisions sit with the buyer. The finish designation, whether an AA code such as M42C21A34, a MIL-A-8625 type and class or a supplier’s own name, needs a sample to define what the words mean on a given line. Every lot also needs the same alloy where the color matters. When a program needs its first anodized lengths approved before volume, low-volume profile extrusion and bridge production are where the rack points, the etch and the color sample are agreed before the first rack goes into the tanks.
Sources and Further Reading
- Premium Anodizing Solutions, Surface Excellence in Europe, 2020, Hydro
- Anodizing Definitions and Methods, Aluminum Anodizers Council
- Current Anodizing Processes, Aluminum Anodizers Council
- Chemical Treatment Prior to Anodizing, Aluminum Anodizers Council
- Anodic Coating Designation System, Aluminum Anodizers Council
- Alloys Suitable for Anodizing, Technical Bulletin 4-13, Aluminum Anodizers Council
- Mechanical Finishing, Aluminum Anodizers Council
- Finding the Right Finish for Architectural Aluminum, Aluminum Anodizers Council
- Interference Coloring, Aluminum Anodizers Council
- ISO 7599:2018, Anodizing of aluminium and its alloys, Method for specifying decorative and protective anodic oxidation coatings on aluminium, sample pages, ISO via SIST’s preview server
- BS EN ISO 7599:2018, Method for specifying decorative and protective anodic oxidation coatings on aluminium, BSI
- Weathering of Anodized Aluminium, Qualanod Technical Information, Edition 03.08.2011, Qualanod
- Product Defects in Aluminum Extrusion and Their Impact on Operational Cost, The 6th Saudi Engineering Conference, Vol. 5, 2002, King Fahd University of Petroleum and Minerals
- Streaking on Aluminium Alloy Extrusions, Master of Engineering thesis, 2012, Auckland University of Technology